ICF10B

externally cooled and lubricated by spraying. The die is normally preheated to a temperature within the range of 150 to 350 °C, depending on the type of casting alloy. For aluminium and brass, the melt temperature is approximately 700 and 970 °C, respectively. During injection, the entrance velocity of the liquid metal is typically within the range of 20 to 60 m/s, but can be significantly lower (1 to 10 m/s) for brass. The metal pressure during injection can exceed 70 MPa. Hot work tool steels, such as AISI H11, H13, H21 and H22, are frequently used as die materials. Thermal fatigue (or heat checking) is an important life-limiting factor in die casting moulds [1-3]. It is a fatigue process caused by the cycling of stress, strain and temperature in the die surface through the thermal cyclic nature of the casting process. Thermal fatigue of die casting moulds is a low cycle fatigue phenomenon basically controlled by the plastic strain imposed on the surface. However, both creep and oxidation may significantly contribute to damage and in some cases they can be the dominant failure mechanisms [4-7]. Thermal fatigue damage is often observed as a network of fine cracks on the surface exposed to thermal cycling. The crack network degrades the surface quality of the tool and, consequently, the surface finish of the cast products, and may eventually cause rejection of the casting. In addition to thermal fatigue cracking, gross fracture, erosion, corrosion and local adherence of the casting alloy (soldering) are other important failure modes which limit the life and performance of die casting dies. Surface engineering is today successfully introduced to improve the erosion and corrosion resistance as well as to reduce soldering of dies and die materials [2, 8-13]. In addition, tests show that surface engineered materials may increase or decrease the resistance to thermal fatigue cracking as compared to an untreated material [11-13]. However, the resistance of surface engineered materials exposed to thermal cycling is not fully explored. To increase the understanding of the thermal fatigue behaviour of surface engineered hot work tool steels exposed to thermal cycling it is necessary to perform experimental simulations. Since thermal fatigue cracks are usually limited to a thin surface layer of the tool, the surface response during the thermal cycling is of particular interest. In this study the following conditions of a hot work tool steel were evaluated: quenched and tempered (reference), treated by boriding and Toyota diffusion (CrC), CrN-coated and duplex-treated (CrN), respectively. The test is based on induction heating and surface strain measurements through a noncontact laser speckle technique. This enables studies of the changes of the response of the surface during thermal cycling. EXPERIMENTAL Materials A hot work tool steel, Uddeholm QRO 90 Supreme, with the nominal chemical composition (wt. %) 0.38 C, 0.30 Si, 0.75 Mn, 2.6 Cr, 2.25 Mo, 0.9 V and Fe bal., was used as test material. The reference specimens were hardened and tempered (austenitizing 30 min at 1030 °C and tempering 2×2 h at 625 °C), followed by fine grinding to a surface roughness of (Ra-value) 0.38 ± 0.05 µm. Prior to surface engineering, the specimens were ground and polished with 1 µm diamond paste in a last step to a surface roughness of (Ra-value) 20 ± 14 nm. The specimens were surface treated by boriding (~25 h at ~850 °C), Toyota diffusion to generate CrC (TDP CrC) (6 h at 1030 °C) or plasma nitriding (15 h at 480 °C), to produce a diffusion zone without any iron nitride compound layer. The boriding process was followed by hardening and tempering (at 1030 °C and 2×2 h at 625 °C, respectively), while the TDP treatment was followed by tempering 2 h at 625 °C and 2 h at 600 °C. All plasma nitrided specimens were duplex-treated with a PVD CrN coating on top of the nitrided layer. The PVD CrN coatings were produced in a multi-arc process, with a deposition temperature of 300 - 400 °C. The five treatments resulted in different mechanical properties, see Table 1. TABLE 1

RkJQdWJsaXNoZXIy MjM0NDE=