ICF10B

Table 1 Results of Fatigue Tests of Co-Fe Specimens Spec. (2) Max Stress ÷ UTS Crack length (a) at bifurcation (mm) (a/b) KI (MPam0.5) at bifurcation (1) Cycles to Failure 1a 0.85 0.93 0.930 65.68 2.04E+04+ 2a 0.78 2.05 0.203 104.58 4.80E+04+ 3a 0.71 1.85 0.183 87.21 9.86E+04+ 5a 0.63 3.40E+06+ (run out) 6a 0.84 1.29 0.128 79.64 1.39E+04+ 7a 0.77 1.39 0.138 76.94 4.67E+04+ 8a 0.74 1.42 0.140 74.33 6.90E+04+ 9a 0.70 3.40E+06+ (run out) 10a 0.63 3.40E+06+ (run out) 1b 0.84 0.60 0.060 50.09 2.81E+04+ 3b 0.76 0.83 0.082 54.88 4.01E+04+ 4b 0.74 0.96 0.095 67.79 6.57E+04+ 5b 0.89 0.55 0.055 51.12 0.52E+04+ 7b 0.92 0.73 0.072 61.77 1.15E+04+ 8b 0.89 0.60 0.060 53.63 1.55E+04+ 13b 0.63 3.40E+06+ (run out) 14b 0.68 0.71 0.070 44.54 6.27E+04+ (1) Based on assumed LEFM behaviour using the formulation presented in reference 1. (2) "a" designates Rotelloy® 7 specimen "b" designates Rotelloy® 8 specimen Fig. 1 Co-Fe Fatigue Specimen