ICF10B

ORAL REFERENCE: ICF100589OR FATIGUE CRACK PROPAGATION OF DISSIMILAR METAL WELDS C.S. Kusko1, J.N. DuPont1, S. Spooner2, and A.R. Marder1 1. Department of Materials Science and Engineering, Lehigh University, Bethlehem, PA 18015, USA 2. Oak Ridge National Laboratory, Oak Ridge, TN 37831, USA ABSTRACT The hard martensite layer that forms adjacent to the fusion line of austenitic/ferritic dissimilar metal welds has been investigated by microstructural characterization and mechanical testing methods. Residual stress measurements were made in the vicinity of the fusion line in both the substrate and overlay materials and fatigue crack propagation tests were performed as to allow the crack to propagate along the dissimilar alloy weld fusion line. This hard martensite layer was found to be non-detrimental to the fatigue crack growth response, as the majority of the fatigue cracks propagated across the martensite layer and fusion line and into the substrate. The compressive residual stresses within the substrate contributed to the enhancement of the growth response of the weld overlay specimens. Based on these results, the hard martensite layer should not be a major factor in causing failure along the fusion line in austenitic/ferritic dissimilar metal weld overlay applications. KEY WORDS fatigue crack propagation; microstructure; martensite; weld INTRODUCTION In the power generation industry, austenitic weld overlays are often used for erosion and high temperature corrosion resistance for ferritic carbon and low alloy steels [1]. Fabrication of such dissimilar metal welds can result in distinct problems. For example, rapid cooling and overlay/substrate chemical composition differences [2] lead to the formation of a martensite layer adjacent to the weld fusion line [3-11]. Figure 1 illustrates a typical martensite layer that forms along the fusion line of a 309L stainless steel/A285 carbon steel weld [11]. Previous research by Kusko [11] has provided a fundamental explanation for the formation of the martensite layer, which leads to steep microstructural and mechanical property gradients across the fusion line. For example, Figure 2 illustrates microhardness results conducted across the fusion line of the 309L stainless steel/A285 carbon steel weld [12]. As evidenced from this figure, the hardness in the martensite layer region can reach values that are approximately twice as large as the hardness values found in the bulk austenitic overlay and ferritic substrate. In addition to this detrimental microstructural gradient, the coefficient of thermal expansion mismatch between the overlay and the base material induces thermal stresses at the fusion line [2]. A post-weld heat treatment (PWHT), which is often incorporated in order to reduce the magnitude of residual stresses, can induce significant microstructural changes and thus, additional gradients in mechanical properties [3]. It is generally known that fatigue crack initiation often occurs more rapidly in welded structures as compared to non-welded structures due to welding defects and other stress concentrators. Consequently, a significant portion of a weld’s fatigue life is spent in the propagation stage. The presence of such weld-related stress concentrators, in addition to the aforementioned hard martensite layer found adjacent to the fusion line, makes fatigue crack propagation a concern for dissimilar metal welds. In addition, residual stresses resulting from welding and

RkJQdWJsaXNoZXIy MjM0NDE=