ICF10B

Unlike the residual compressive modulus, the residual compressive strength reveals an 11 % on average knockdown due to HC conditioning alone. Damage associated with the HC conditioning may have a greater influence on the extreme values of a defect population (size, spacing) effecting strength, while having an indistinguishable influence on the average distribution of flaw characteristics effecting modulus. Indeed Lacy, McDowell, Willice and Talreja [7] show that different damage distributions may exhibit identical stiffness properties while having markedly different rates of damage evolution and tolerance to damage. The residual compressive strength of the 0 hr and 12k hr datasets are intermingled with the accumulation of mechanical fatigue. This is in spite of clear differences in the observed failure morphologies for the two datasets. Upon static failure, the 0 hr samples generally revealed clean transverse fractures, with only modest ply delamination at the most aggressive states of fatigue damage. In contrast, the 12k hr HC conditioned material revealed extensive delamination, both at the ply and bundle interfaces. This strongly indicates that the damage induced by the HC missions was most degrading to the fiber/matrix interface. Fig. 10 takes the final step of comparing the compressive residual strengths with the corresponding residual compressive modulus values. Presentation of the fatigue data in this manner is believed to be relatively unique; empirically it infers a proportional relationship between residual strength and modulus. First, it can be stated that each of the datasets independently suggests a consistent relationship between these two properties. Furthermore the 0 hr data are layered above the 12 khr data with the similar proportionality. While the 0 hr and 12 khr material may exhibit similar compressive modulus response, the residual compressive strength of the 0 hr material tends to be greater. This relationship will be further examined with additional conditioning times ranging to 30k hours of the HC exposure. CONCLUSIONS In conclusion, an experimental investigation was conducted to examine the fatigue damage progression and damage tolerance of a high temperature graphite/epoxy PMC under fully reversed axial loading conditions with and without hygrothermal cycle conditioning. The specimen geometry performed well at elevated temperature without anti-buckling guides for fully–reversed fatigue and compressive strength testing. A deterministic relationship was found between the applied stress range and the number of cycles to failure; the resulting stress-life data in Fig. 6 maybe used to make design life predictions. Prior to mechanical fatigue loading, the 12 khr material experienced an 11 % strength degradation relative to the 0 hr material. No distinction was found between 0hr and 12 khr material when examining the residual compression modulus and residual compression strength as a function of fatigue cycle. Designers may find that the correlation of residual compressive strength and modulus in Fig. 10, give a clearer representation of compressive strength degradation due to HC conditioning. Evaluation of 30 khrs conditioned material is in progress to verify this trend. ACKNOWLEDGEMENTS The authors acknowledge Chris Burke for technical assistance in the laboratory, Rod Ellis for project guidance and oversight, and also Ron Cairo, Rajiv Naik, and Ken Tosi of Pratt & Whitney for numerous interactions on the project. The work was made under the NASA cooperative research grant NCC3-821. REFERENCES 1. Cornelia., D.(1994). In: 39th International SAMPE Symposium, pp. 917-929. 2. Bakis, C.E. et al. (1989). In: Composites (2nd Vol), ASTM STP 1003, pp.180-193. 3. Gyekenyesi, A.L. (1998). ASME-98-GT-106. 4. Talreja, R. (1981). In: Proceedings of the Royal Society of London, A378, pp. 461-475. 5. Nilsson, K. F., Thesken, J. C., Sindelar, P., Giannakopoulus, A. E. and Storåkers, B. (1993) J. Mech. Phys. Solids 41, 749-782.

RkJQdWJsaXNoZXIy MjM0NDE=