clear that simple superposition of initial tensile residual stress onto applied far-field stress provides a significant contribution to the reduction in fatigue life due to FOD through its effect in elevating the local Rratio. Threshold conditions based on the Kitagawa diagram For high applied stress ranges (relative to the magnitude of tensile residual stresses) and in the presence of relatively large impact-induced microcracks (~ 30 to 50 µm), it was found that fatigue failures at 105 to 106 cycles initiated directly at the impact site. These fatigue failures (shown as closed symbols in Fig. 6) have been described in our previous work [5] through the use of fatigue crack growth threshold concept and the Kitagawa-Takahashi diagram [11]. Here, the limiting threshold conditions were defined by the stressconcentration corrected smooth-bar fatigue limit (at microstructurally-small crack sizes) and a “worst-case” fatigue crack growth threshold (at larger “continuum-sized” crack sizes). A more favorable representation of the failure envelopes for the two load ratios of 0.1 and 0.5 in Fig. 10 can be made using the El Haddad et al. [12] empirical quantification of Kitagawa approach, which introduces a constant, termed the intrinsic crack length, 2co, such that the stress intensity is defined as ∆K = Y ∆ σ [ π (2c + 2co)] ½, where Y is the geometry factor. To account for residual stresses in this approach to describe the limiting threshold conditions for FODinitiated HCF failures in Ti-6Al-4V, the effective R-ratio in the diagram has to be corrected for the presence of such residual stresses. Using the fatigue failures plotted in Fig. 10 as data points at surface crack lengths of 2c = 1 µm, and superimposing the measured tensile residual stress of ~300 MPa, the R-ratios are increased from 0.1 to ~0.5 and from 0.5 to ~0.7 at far-field stress range of ~300 MPa. Accordingly, such failures at both load ratios can still be described by the proposed Kitagawa-Takahashi approach, provided the limited conditions are given by the stress concentration and residual stress corrected smooth-bar fatigue limit at small crack sizes and the “worst-case threshold” for larger crack sizes. The full quantitative effect of the FOD-induced residual stresses on fatigue failures at 105 to 106 cycles, however, is still under study. Although simple superposition of the residual and applied stresses was considered above, our recent in situ x-ray micro-diffraction results have indicated that during the first few fatigue cycles, significant relaxation of the residual stresses occurs at the base and rim of the impact crater, but not at locations a crater diameter or so away where fatigue cracks initiate under low applied stresses. This effect is currently under investigation using both in situ x-ray studies and numerical computation. Laser Shock Peening Laser shock peening (LSP) has been proposed as an effective means to improve the fatigue strength of titanium turbine blades, especially to enhance the HCF resistance to FOD [1,8]. A prime cause for this effect is that LSP can induce significant compressive residual stresses below the surface, which inhibits the propagation of FOD-related surface fatigue cracks. The positive effect of LSP prior to 200 m/s (3.2 mm shot) impacts is shown in Fig. 7, where it can be seen that the LSP process resulted in fatigue life extension of more than one order of magnitude. However, at higher impact velocities of 300 m/s (3.2 mm shot), LSP had little influence on HCF resistance (Fig. 7). As the impact crater sizes were essentially identical for non-LSP and LSP treated fatigue samples at this velocity, the similar fatigue lives appear to be the result of the deep impact penetration compared to the depth of LSP-induced compressive residual stresses. Currently, both experimental and numerical studies are focused on quantifying residual stress gradients after the LSP process and following FOD in order to explain limited benefits of LSP for the high velocity impacts. SUMMARY AND CONCLUSIONS Based on a study of the role of foreign object damage in affecting the high-cycle fatigue of an engine Ti-6Al4V alloy with bi-modal microstructure, the prominent conclusions are: 1. Foreign object damage, simulated by high-velocity (200-300 m/s) impacts of steel spheres (1 and 3.2 mm shot) on a flat specimen surface, markedly reduced the HCF resistance, primarily by inducing sites for the premature initiation of fatigue cracks on subsequent cycling. 2. Premature crack initiation was caused by a number of factors: (i) the stress concentration due to the FOD indentation, (ii) the creation (at highest impact velocities only) of microcracks at the impact crater rim, (iii) microstructural damage from FOD-induced plastic deformation, and (iv) the localized presence of tensile residual stresses around the indent. 3. Two groups of FOD-induced HCF failures could be identified. The first group involved fatigue crack initiation directly at the impact site and caused failures within 105 to 106 cycles. The proposed criteria for such failures has been described by a modified Kitagawa-Takahashi approach, where the limiting threshold conditions are defined by the stress-concentration corrected smooth-bar fatigue limit (at
RkJQdWJsaXNoZXIy MjM0NDE=