EXPERIMENTAL Binary blends of a star block copolymer (ST2-S74) and a triblock copolymer (LN4-S65), both based on styrene and butadiene, are used in this study. The characteristics of the block copolymers are given in table 1. After mixing the materials in extruder, the single-edge notched bend (SENB) specimens were prepared by injection molding (mass temperature 250°C and mold temperature 45°C). The blends contain 5, 10, 20, 40, 60 and 80 wt % of LN4-S65. Table1: Characteristics of the blend components; styrene as hard outer block in LN4 is 32 vol. % while the middle statistical block contains about 50 vol. % styrene. blend component Mn (g/mol) Mw/Mn Φstyrene Morphology (TEM) ST2-S74 109,200 1.69 0.74 lamellar LN4-S65 116,000 1.20 0.65 PS domains in S/B copolymer matrix In order to quantify the toughness behavior of investigated block copolymer blends, an instrumented Charpy impact tester IKBV-4J with 4J total work capacity was used. The SENB specimens have following dimension: length L = 80 mm, width W = 10 mm and thickness B = 4 mm. The specimens were notched with a razor blade (notch tip radius = about 0.13 µm). For the measurement of fracture mechanics parameters as resistance against unstable and stable crack growth, the initial crack lengths of 2 mm and 4.5 mm were cut [8]. To minimize the vibration of specimen, the span length was set to 40 mm, and the pendulum hammer speed was 1m/s. The determination of Young’s modulus and yield strength as well as the fracture mechanics parameters as resistance against unstable crack initiation is carried out by using the procedures described in ref. [8]. Because blends with LN4 content ≥ 20 wt % reveal stable crack propagation behavior, an equivalent toughness characterization of these blends was only possible by crack resistance (R-) concept of elastic-plastic fracture mechanics. Crack resistance curves (R-Curves) represent the functional dependence of loading parameters (J-integral or δ) with the stable crack growth ∆a. These curves allow the determination of fracture mechanics parameters as resistance against stable crack initiation and propagation. The multispecimen-method in the stop-block-technique is found to be most effective for polymeric materials. Further details on determination and evaluation of R-curves under impact loading conditions are discussed in [8]. A small piece of each sample was cut from the bulk specimen and immersed in an aqueous osmium tetroxide (OsO4) solution for several hours at room temperature to selectively stain the butadiene phase. Ultra-thin sections were cut using an ultramicrotome (Reichert Ultracut E) equipped with a diamond knife (Diatome). Microphase morphology of the samples was examined using a 200 kV transmission electron microscope (TEM, JEOL 2010). In order to correlate the microstructure and fracture behavior with micromechanical deformation behavior, fracture surfaces of the specimens were qualitatively as well as quantitatively analyzed by scanning electron microscope (SEM, Jeol JSM-6300). Special attention was paid to quantification of some selected areas on the fracture surfaces like crack-tip blunting zone (stretch zone). For this purpose, the fracture surface of the SENB specimens were mounted on 45° sloped specimen target and sputtered with gold prior to the SEM imaging. RESULTS AND DISCUSSION Samples ST2 and LN4 have equilibrium morphologies comprising of alternating lamellae and randomly distributed cylinders [9] respectively. Morphology of the block copolymers and their blends is strongly influenced by shear stress of injection molding. As shown in fig. 1, lamellar structures of sample ST2 are aligned parallel to the injection direction by the shear stress.
RkJQdWJsaXNoZXIy MjM0NDE=