ICF10B

ICF100489OR FRACTURE MECHANICS MODELS FOR THE ANALYSIS OF COMPOSITE MATERIALS WITH A NONLINEAR MATRIX A. Carpinteri, G. Ferro & G. Ventura Department of Structural Engineering, Politecnico di Torino, 10129, Torino, Italy. ABSTRACT A model for reproducing the constitutive flexural response of a fiber-reinforced composite material with a non-linear matrix is proposed. The nonlinearity of the matrix is modelled by considering a distribution of closing forces onto the crack faces which increases the fracture toughness of the cross-section with a shielding action. The constitutive flexural response depends on three dimensionless parameters: ˜wE c , which controls the extension of the process zone, N (1) P and N (2) P , called brittleness numbers, which are related to the reinforcement phases. The role of the specimen size scale is fundamental for the global structural behaviour, which can range from ductile to brittle simply with the variation of the two brittleness numbers. They are functions of matrix toughness, reinforcement yielding or slippage limit, reinforcement volume fraction and global structural size. The application of the model to steel bar reinforced high-performance concrete with fibers is in good agreement with the experimental results. KEYWORDS Fracture mechanisms, Fiber-reinforced composite material, High-performance concrete, Bridged crack, Size effects. INTRODUCTION The development of high-performance composite materials has been playing a key role in the recent engineering applications. In civil engineering, for example, the introduction of high-strength concretes, characterized by a very brittle behaviour, has required the addition of a secondary phase of reinforcement (fibers) to increase the fracture toughness of the material, so that the cementitious matrix assumes a nonlinear constitutive behaviour. The development of high-performance concretes is emblematic for the modern approach to new composite materials. Despite a large proliferation of experimental tests and papers on the structural behaviour of reinforced elements, there are not theoretical models which describe in exaustive manner these materials. The purpose of this paper is to offer a contribution to the theoretical modelization of the bent elements. The application of Fracture Mechanics concepts to plain and reinforced concrete structures represents the only way to interpret the collapse behaviour, which shows different rupture modes by varying the size. Two different models have been proposed in the last few years to describe partial damage near a single crack: the cohesive crack model and the bridged crack model. In the former, the stress-intensity factor KI at the crack tip is set equal to zero due to the contribution of the applied load and of the softening tractions acting ahead of the notch. The first application to brittle materials is due to Barenblatt [1], while important contributions to relate the cohesive model to the Griffith crack are due to Willis [2] and Rice [3]. In the bridged crack model the near tip process is modeled via the stress-intensity factor and a crack propagation condition is reached when the stress-intensity factor equals the toughness of the brittle matrix. Several bridged crack models have been proposed to simulate the structural response of fiber-reinforced materials. These models have been used to describe cracking in brittle-matrix composites [4] and in alloy plates shielded by bonded patches [5], as well as damage zones in concrete [6]. The theoretical model to which we refer determines the problem unknowns by considering the cracked crosssection and by using the local compliance and the stress-intensity factor concepts. It represents an extension of the model proposed by Carpinteri [7] for one single reinforcement, by Bosco and Carpinteri [8] for a discontinuous fiber distribution and by Carpinteri and Massabo` [9] for a continuous distribution. The longitudinal

RkJQdWJsaXNoZXIy MjM0NDE=