ICF10C

C) Figure 2. Figure 2. Crack contours in the steel plates exposed to cathodic charging with uniaxial stress. / o = 0.052; b) / o = 0.2 and c) / o = 0.5 0 5 10 15 20 25 30 0.042 0.186 0.452 s / so number of cracks first inspection total cracks performed Figure 4. Number of detected cracks during the HIC test. Figure 5. Examples cracks linking in a stepwise manner, observed in the loaded plates.