ICF10B

an increase of the stress amplitude during strain-controlled cyclic loading. Since this stress increase retains until failure, the cyclic stress-strain curve (css curve) is shifted upwards by predeformation (prehistory dependent behaviour). As opposed to planar-slip materials, simple and general statements are not possible for materials showing wavy dislocation glide. The behaviour is determined not only by the extent of predeformation, rather the amplitude of the subsequent cyclic loading plays also a significant role. Tendentiously the dependence on a mechanical prehistory ceases at a small predeformation in combination with high plastic strain amplitude. It should be noted in this context that the term prehistory dependence relates only to the mechanical behaviour. As shown in [4], very similar stress-strain responses may result from different types of dislocation arrangements formed during cycling without and after predeformation, respectively. The results presented are part of a comprehensive study aimed at a detailed understanding of the influence of a monotonic room-temperature predeformation on the high-temperature fatigue behaviour of nickel-base alloys [5]. The emphasis in this paper is put upon cyclic lifetime effects. A simple parameter is introduced which allows to quantify the degree of the influence of relevant loading parameters on both the cyclic stressstrain response and fatigue life and therefore applies to a prediction of predeformation-induced changes in the number of cycles to failure Nf. Microstructural aspects are only dealt with as far as they help to define the applicability range of this predeformation parameter. More details on the microstructural and mechanistic aspects are given in [6]. EXPERIMENTAL DETAILS The materials studied were two polycrystalline nickel-base alloys, Nimonic 75 and Nimonic 105, which were tested in three different precipitation conditions. Nimonic 75 is a precipitate-free nickel-base superalloy and was used to represent the behaviour of the matrix of Nimonic 105 (precipitate-free condition). In order to improve the comparability to this particle-strengthened material, the mean grain size of Nimonic 75 was adapted to the one of Nimonic 105 by means of an annealing treatment that led to a mean grain size of 60µm. Nimonic 105 was used in two different heat-treated conditions. After a solution annealing with subsequent water quench, an ageing at 850°C for 16 hours was applied to establish the peakaged condition that corresponds to the hardness maximum at RT. The over-aged condition resulted from an annealing at 1000°C for 500 hours. The peak-aged condition is characterised by spherical γ' precipitates of a mean particle diameter of 73 nm at a volume fraction of 43%. The over-ageing treatment led to a γ' volume fraction of 38%. In this condition, the γ' precipitates were present in three superimposed size distributions with mean sizes of 32nm, 138nm and 665nm. As a consequence of the existence of small precipitates in the over-aged condition, the cyclic deformation behaviour of both conditions was found to be very similar and will therefore be reported jointly. Specimens with a cylindrical gauge length of 6mm in diameter were tested in an electrohydraulic servocontrolled test system equipped with high frequency heating. The fatigue tests were performed at room temperature (RT), 400°C, 600°C and 800°C. True plastic strain control in combination with a triangular command signal was applied in all fatigue tests in such a way that the plastic strain rate was held constant at a absolute value of 5⋅10-4 s-1. Plastic strain amplitudes ∆εpl/2 ranging from 0.025% to 0.25% were used and were kept constant throughout the test (irrespective of a continuous change in Young´s modulus E) by means of a superimposed control of the plastic strain value at zero stress. Figure 1: Effect of tensile predeformation on position of hysteresis loop

RkJQdWJsaXNoZXIy MjM0NDE=