the main reason why the SP_SWT concept introduced by Figure 7 applies to this material as well. However, the dislocation arrangement in copper as a wavy-slip metal depends very sensitively on the plastic strain amplitude of cyclic loading and the degree of predeformation. Dislocation cells are formed at high values of ∆εpl/2, but are also prevailing after strong prestraining and subsequent cyclic deformation even at low ∆εpl/2. Single-slip dislocation arrangements, such as bundle/vein structure and persistent slip bands, are restricted to small value of ∆εpl/2 and very low degrees of predeformation. Taking this strong variation in dislocation arrangement into account and considering that the SP_SWT parameter ignores changes in microstructure and mechanism, it is not surprising that the data of copper can not be described by a single curve in the representation of the cyclic life ratio versus SP_SWT. Consequently, a prerequisite for the application of the SP_SWT concept is that no fundamental changes in the microstructure takes place within the range of predeformation and cyclic loading parameters considered. CONCLUSIONS The main results obtained in this study on the effect of a monotonic tensile prestrain on cyclic stress-strain response and fatigue life of Nimonic 75 and Nimonic 105 (over-aged and top-aged) at temperatures ranging from room temperature up to 800°C can be summarized as follows: • The effect of predeformation on cyclic life can be described by means of the Smith-Watson-Topper damage parameter PSWT despite a change in the microstructure and the favourable crack initiation site with room-temperature tensile prestraining • Based on PSWT the predeformation parameter d predeforme SWT d not predeforme SWT P SWT P P S = −1 _ is introduced. • SP_SWT successfully applies to quantitatively describe the effect of cyclic loading parameters, extent of predeformation and particle strengthening on the prehistory dependence. • SP_SWT correlates with the predeformation-induced cyclic life change in an unambiguous way. This correlation is independent of the temperature of cyclic loading. • The applicability of SP_SWT is restricted to materials and conditions which do not undergo a fundamental microstructural change. Acknowledgement: The authors gratefully acknowledge financial support of this study by Deutsche Forschungsgemeinschaft. REFERENCES 1. Feltner, C. E. and Laird C. (1967) Acta met. 15, 1612-1632 and 1633-1653. 2. Lukáš, P. and Klesnil M. (1973) Mater. Sci. Engng 11, 345-356. 3. Coffin, L. F. (1967) Trans. ASME 60, 160-175. 4. Hoffman, G., Öttinger, O. and Christ H.-J. (1993). In: Proc. Low Cycle Fatigue and Elasto-Plastic Behaviour of Materials (LCF3), pp. 106-111, Rie, K. T. (Ed.). Elesvier Applied Science, London. 5. Schöler, K. (1999) Einfluß der Mikrostruktur auf das Wechselverformungsverhalten teilchengehärteter Legierungen bei hohen Temperaturen nach einer Vorverformung. Doctorate Thesis, Universität Siegen. 6. Schoeler, K. and Christ, H.-J. (2000) Intern. J. Fatigue, in print 7. Gerold, V. and Karnthaler, H. P. (1989) Acta met. 37, 2177-2183 8. Zheng, D., Rosenberg, A. and Ghonem, H. (1993) Mater. Sci. Engng A161, 13-21. 9. Smith, K. N., Watson, P. and Topper, T. H. (1970) Journal of Materials, JMLSA 5, 767-778. 10. Nihei, M., Heuler, P., Boller, Ch. and Seeger, T. (1986) Intern. J. Fatigue 8, 119-126. 11. Hoffmann, G. (1996) Wechselverformungsverhalten und Mikrostruktur ein- und mehrphasiger metallischer Werkstoffe nach einer Vorverformung, Doctorate Thesis, Universität Erlangen-Nürnberg
RkJQdWJsaXNoZXIy MjM0NDE=