EXPERIMENTAL Al-6061 matrix alloy powders (Al-0.27 Cu-0.26 Fe-0.97 Mg-0.56 Si)2 were initially screened to -325 mesh prior to blending with the SiC reinforcement. During the blending stage, the matrix and reinforcement powders were suspended in a slurry using 1-butanol as the solvent, in order to reduce agglomeration due to electrostatic forces. After blending, the powders were carefully dried, re-screened to -325 mesh and placed in an extrusion can. An elevated temperature vacuum de-gas treatment was used to remove all traces of residual solvent from the powders, before sealing the cans for compaction and extrusion. Extrusion was carried out at 450˚C, with an extrusion ratio of 25:1 (round : round), followed by an air cool (F-temper designation). Particle aspect ratios were measured from digital micrographs, using a commercial desktop image analysis package3. Around 200 particles were selected from each micrograph, at random, in order to perform a statistical analysis of the particle aspect ratios in each material, in both transverse and longitudinal orientations with respect to the extrusion direction. Particle size statistics for the as-received powders were obtained using a Coulter LS 230 Particle Size Analyzer, with small volume unit and associated software. Duplicate samples of each reinforcement were analyzed, using ethanol as the suspension medium. Room-temperature tensile testing was carried out using a servo-hydraulic test frame under displacement control at a constant strain rate of 1.3 x 10-4. A flat dog-bone specimen with a gauge length of 25.4 mm was used throughout. The oversize specimen ends were gripped between hydraulic jaws, and a clip-on extensometer was attached to the larger specimen faces for strain measurement. Each specimen was loaded to failure. The two specimen halves were then carefully separated and set aside for examination in SEM. RESULTS Microstructural Characterization Figures 3(a) and 3(b) show longitudinal sections through each microstructure, with the extrusion direction horizontal. The two microstructures are very similar; especially in terms of the homogeneity of the spatial distribution of SiC particles. However, the F-600 material clearly contains a wider distribution of particle sizes, with many small, angular particles in the section. This qualitative statement agrees well with the particle size analysis results for F-600 SiC ( d p = 12.0 µm, s.d. = 4.0 µm) and HBD SiC ( d p = 11.5 µm, s.d. = 3.0 µm), in the as-received condition. No obvious porosity was observed in either microstructure. 2 spherical gas-atomized 6061-Al powder, obtained from Valimet, Inc. CA. 3 Adobe Photoshop 5.5, running Image Processing Tool Kit, v2.10. (a) (b) 100 µm 100 µm Fig. 3: Typical microstructures of (a) F-600 and (b) HBD DRA materials. Longitudinal sections, F-temper, unetched (extrusion direction is horizontal).
RkJQdWJsaXNoZXIy MjM0NDE=