ICF10B

effects of gaseous environments other than oxygen and hydrogen have not been studied extensively. Shimojo et al. [2] reported that fatigue crack growth rates of titanium increased in a pure nitrogen environment as compared to that in vacuum. Nitrogen is considered to be less aggressive than oxygen, but it can still react with titanium and, thus, could inhibit reverse slip. Though it is generally considered that noble gases do not affect fatigue crack growth, it is also shown that even noble gas environments can affect fatigue crack growth rate of pure titanium. Shimojo et al. [3, 4] showed that noble gas such as pure helium, argon and xenon increased fatigue crack growth rate as compared to that in vacuum. Fatigue crack growth rates in helium, argon and xenon were approximately twice that in vacuum and were almost the same as that in air. Additional findings showed that striations were clearly observed on fracture surfaces of specimens tested in helium and xenon, while less obvious striations were observed on those in vacuum and argon. These interesting results indicate that even noble gases may adsorb strongly on exposed slip steps and affect fatigue behaviour of titanium. However, most fatigue data obtained in noble gases, to date, are treated as reference data for more aggressive environments. Very little research has been carried out on the effects of noble gases themselves on fatigue behaviour of metals. Thus, the mechanism causing these effects of noble gases is still uncertain. Noble gas atoms are less likely to form a strong bond with metals. But, on the other hand, titanium is a reactive metal, which means that titanium atoms form a bond easily with other atoms. The above-mentioned effects of noble gases on fatigue crack growth may result from the active nature of titanium and may appear on other titanium alloys, not limited to pure titanium (α-titanium, hcp structure). In this research, fatigue crack growth tests are carried out on a β-titanium alloy, which has a bcc structure, in noble gases and the effects of noble gas environments on fatigue crack growth behaviour are discussed. EXPERIMENTAL PROCEDURE The material used was a hot-rolled and annealed β-titanium (Ti-15V-3Al-3Cr-3Sn) polycrystalline plate. This material has a microstructure that consists of equiaxial grains, the diameter of which was approximately 150 µm. Compact tension specimens of 50 mm width and 12.5 mm thickness were prepared from the material with an L-T orientation (the macroscopic crack plane is perpendicular to the loading direction, and the crack growth direction parallels to the transverse direction of the plate.) Fatigue crack growth tests were performed under a sinusoidal loading control at a frequency of 10 Hz and a stress ratio of 0.1 using a servohydraulic fatigue machine with an environmental chamber made of stainless steel. The block diagram of the measurement system is shown in Fig.1. Crack length was monitored using a direct current potential drop technique. Some tests were carried out under constant load amplitude conditions and others were under constant stress intensity factor range (∆K) conditions by feeding back the crack length measured. All tests were carried out at room temperature (approximately 24oC) in an environment either vacuum or high purity noble gas of 1 x 105 Pa. Attention was paid especially to the purity of the gases and the contamination that might have occurred during the introduction of the gases to the chamber. (The effects of air contamination on fatigue crack growth rate and on fracture surface

RkJQdWJsaXNoZXIy MjM0NDE=