increasing Vc, however, crack growth rate effect dominates after Fmax. On the other hand the constant load test shows an increasing Vc from beginning of the test onwards as expected. CONCLUSIONS The microstructure influences the deformation and creep behaviour of TiAlCr alloys. The fracture mode in CT specimens at 700°C is brittle with microcracking observed in γ-phase and along lamellar interfaces. Large discrepancy, up to 50 per cent, between crack lengths measured on fracture surfaces and those determined using DCPD method were caused by unbroken lamellar ligaments, and crack branching and crack tunneling. EDM slit notches with tip radius of 0.05mm can be used as sharp starter cracks. Creep crack growth tests can be done both under constant load and displacement rate control provided the effects of crack growth on stress state is accounted for. Crack growth data from displacement rate controlled tests beyond maximum load (Fmax) may not be correlated with crack tip parameters. The data from transition range i.e. ∆a<0.2mm may be correlated with K. The time dependent crack growth data assessed following the ASTM standard [11] correlates with C*(t). However, much work is needed particularly for starter sharp crack requirement, crack length measurements and validity of data in order to assess the components made of creep brittle intermetallics. ACKNOWLEDGEMENTS The author would like to thank B. Petrovski for motivating discussions and scientific support and J. Granacher of T.U.Darmstadt for carrying out creep tests. REFERENCES 1. Kim, Y.-W. (1995) Proc. Symp. Gamma Titanium Aluminides, Y.-W.Kim, R.Wagner and M.Yamaguchi Eds., TMS. Warrendale, Pa.,USA, pp. 637-654. 2. Appel, F. and Wagner, R. (1998) Materials Sci. and Engg., R22 (5), 187-268. 3. Yamaguchi, M., Inui, H. and Ito, K. Acta Mater. 2000, 48, pp.307-322. 4. Kim, Y.-W. JOM, TMS, 1995, 39-41. 5. Dogan, B. (2000) Proc. Int. Conf. Life Assessment of Hot Section Gas Turbine Components, 1999, R.Townsend et.al. Eds. IOM Book B731, pp.209-227. 6. Dogan, B., Schöneich, D., Schwalbe, K.-H. and Wagner, R. (1996) Intermetallics, 4 (1), pp.61-69 7. Dogan, B. and Schwalbe, K.-H. (1997) Engineering Fracture Mechanics, 56 (2), pp.155-165. 8. K.S.Chan and Y.-W.Kim, Met. Trans.A, 1993, 24A, pp.113-125. 9. Fuji, A., Tabuchi, M., Yokobori Jr., A.T. and Yokobori, T. (1999) Engineering Fracture Mechanics, 62 (1), pp.23-32. 10. VAMAS (Varsailles Project on Advanced Materials and Standards) TWA19: High Temperature Fracture of Brittle Materials, 1993-1998. 11. ASTM E1457-98, (1998), Standard Test Method for Measurement of Creep Crack Growth Rates in Metals. Annual Book of ASTM Standards, Philadelphia, 03.01., pp.1031-1034. 12. ASTM E399-90, (1990), Standard Test Method for Plane-Strain Fracture Toughness of Metallic Materials, Annual Book of ASTM Standards, 03.01., April 1991, pp.485-515. 13. ASTM E647-95, (1995), Standard Test Method for Measurement of Fatigue Crack Growth Rates, Annual Book of ASTM Standards, 03.01., April 1995, pp.485-515. 14. Saxena, A. Hall, D.E. and McDowell, D.L., (1999) Engineering Fracture Mechanics, 62, pp.111-122. 15. Kwon, O., Nikbin, K.M., Webster G.A. and Jata, K.V. (1999) Engineering Fracture Mechanics, 62, pp.155-165.
RkJQdWJsaXNoZXIy MjM0NDE=