ICF10B

IHE: Considerations of the kinetics of KTH and da/dt vs dK/dt for IHE in Ti-15-3 suggest that H diffuses rapidly during loading and over a short distance (0.5-5 mm) through b in the fracture process zone to reach the a/b interface [3]. While brittle TiH may form in a [34], hydrides are less important in b alloys due to the high solubility of H in bcc Ti (~15,000 ppm at 25oC) [19,20]. H is enriched in b when a precipitates are present; local hydriding of a, at the interface with b, should occur for total CH above 2500 ppm [19,20]. This hydriding was not observed experimentally and is not a likely cause of cracking at the CH levels in Figure 3. The effect of locally high interface stresses on hydride precipitation is uncertain and this mechanism cannot be discounted. Fracture without H occurs at a/b interfaces in STA alloys such as Ti-15-3. It is reasonable to speculate that this fracture mode is promoted by H, trapped at this interface and with locally high tensile stresses, as envisioned in classic decohesion theory [30,31]. The aging dependence of TG IHE may be understood based on the need for a critical amount of intragranular a. Considering Figure 3, a precipitation was restricted to b-grain boundaries during 0-5 h of aging (a volume fraction of 0 to 0.48) and when Ti-15-3 was immune to IHE. H cracking correlated with a precipitation within many b at the 6 h age (0.52 a) and within all grains at 10-12 h (0.68-0.80 a) [3]. A critical amount of a in b may be required for: (1) a connected path for H cracking [35], (2) locally high tensile stresses from microscopic constraint adjacent to the a/b interface, or (3) H enriched in b and trapped at the interface with a. A connected crack path is not sufficient for IHE since the immune microstructures in Figure 3 exhibited a on all grain boundaries, but IG cracking did not occur. HEE: Metallurgical variables could promote intergranular HEE by enhancing H production and uptake near b-grain boundaries at the crack tip, and by enabling brittle cracking of H-enriched boundaries within the process zone. Two factors constrain the governing metallurgical variable. The fully-IG fracture mode observed for susceptible STA BetaC (Figure 4) dictates that the HEE mechanism and variable must operate at essentially every grain boundary, at least for some b-Ti alloys. Second, since H damage appears to occur within 0.1-1 mm of the crack tip surface contacting NaCl solution, the metallurgical variable must be sized and interconnected on this length scale [25,32]. Three microstructural factors may be consistent with these constraints and change during isothermal aging of the ST-b phase: grain boundary a, slip localization, and elemental segregation. A study isolated these candidate explanations of aging-dependent HEE for the situation represented in Figure 4, but the results were not conclusive [36]. Two features, grain boundary a and H-enhanced slip localization, are not the cause of IG HEE in Beta-C stressed in NaCl solution. TEM and SEM analyses showed that a decorated less than 5% of the b-grain boundaries, but HEE was nearly-100% IG. High magnification examination of matching surfaces of IG facets, using an SEM with a field-emission gun and dual detectors to optimize topographic contrast and resolution, failed to evidence localized plasticity of the sort reported for IG IHE of b/a-Ti [19,20] and hydrogen embrittlement in general [33]. As illustrated by the high-magnification SEM fractograph in Figure 4, the only features resolved were perturbations of the cracked b-grain boundary surface by intersection of occasional a plates. The predominant feature was mildly undulating and featureless grain surfaces, consistent with interface decohesion. Circumstantial evidence suggested that solute segregation to b-grain boundaries during aging, combined with trapped H, explained the onset of IG HEE in b/a-Ti (Figure 4). A similar explanation was adopted for IG IHE of STA Beta-C [20] and H embrittlement of steels [31]. Results implicated segregated Si as reducing boundary cohesion in b-Ti without H [37]. Experiments, where STA Beta-C was aged at higher temperatures to progressively dissolve a and remove segregation, support the importance of elemental segregation [36]. For example, a double aged and a-free microstructure was susceptible to IG HEE, confirming that grain boundary a and intragranular a are not required for embrittlement. Double aging at higher temperatures and longer times eliminated IG HEE in the all-b microstructure and restored the original ST immunity to cracking. The hypothesis was that HEE was precluded by elimination of boundary segregation, due to either reduced thermodynamic driving force or formation of (Ti,Zr)5Si3. Boundaries in HEE-immune and susceptible single and double ages of Beta-C were examined by small-probe STEM. No segregant was observed to correlate with the IG cracking tendency. Auger spectroscopy of intergranular facets produced by in situ fracture of H-precharged STA Beta-C failed to resolve segregation that correlated with severe IG IHE in long time single-aged specimens [20]. Similar aging times and a precipitation are required to trigger IHE and HEE of ST b-Ti, as shown by the similar KTH relationships in Figures 3 and 4. As such, the mechanisms for these aging dependencies of TG vs IG H embrittlement may share a common feature. Elemental segregation to a/b interfaces during aging has not been considered for TG IHE, and enhanced-H trapping from enrichment in b or stress localization due to the presence of a have not been considered for IG HEE.

RkJQdWJsaXNoZXIy MjM0NDE=