CONCLUSIONS 1. The outstanding strength capability of a-precipitation hardened b-Ti alloys is compromised by low plane strain fracture toughness compared to martensitic steels, and by both IHE and HEE. 2. All-b alloys are immune to hydrogen embrittlement for low to moderate H concentrations, but transgranular IHE (along a/b interfaces) and intergranular HEE (along b-grain boundaries) are triggered by a critical amount of aging to form a. 3. Increased strength does not explain the deleterious effects of aging on H embrittlement. The onset of TG IHE appears to be related to H enrichment in b and stress intensification at a/b interfaces continuous through b grains. For IG HEE, neither grain boundary a nor deformation localization explain the effect of aging. Segregation may be the requisite for IG cracking, but offending species were not resolved. ACKNOWLEDGEMENT This research was supported by the Office of Naval Research (Grant N00014-91-J-4164), with Dr. A. John Sedriks as Scientific Monitor. The author acknowledges the critical contributions of B.P. Somerday, S.P. Hayes and L.M. Young, as well as the collaboration with J.R. Scully. REFERENCES 1. Boyer, R.R. and Rosenberg, H.W. (1984). Beta Titanium Alloys in the 80’s, TMS, Warrendale, PA. 2. Eylon, D., Boyer, R.R. and Koss, D.A. (1993). Beta Titanium Alloys in the 90’s, TMS, Warrendale, PA. 3. Hayes, S.P. (2000). PhD Dissertation, University of Virginia, Charlottesville, VA. 4. Young, L.M. (1993). MS Thesis, University of Virginia, Charlottesville, VA. 5. Young, G.A. (1993). MS Thesis, University of Virginia, Charlottesville, VA. 6. Somerday, B.P. (1998). PhD Dissertation, University of Virginia, Charlottesville, VA. 7. Kolman, D.G. (1995). PhD Dissertation, University of Virginia, Charlottesville, VA. 8. Gaudett, M.A. (1997). PhD Dissertation, University of Virginia, Charlottesville, VA. 9. Headley, T.J. and Rack, H.J. (1979) Metall. Trans. A 10A, 909. 10. Shen, G.Q., Wang, S.H., Liang, T.M., Luo, G.Z. and Xie, L.Y. (1996) Trans. Metal Heat Treatment 17, 10. 11. Haynes, M.J. and Gangloff, R.P. (1997) J. Testing Eval. 25, 82. 12. Froes, F.H., Chesnutt, J.C., Rhodes, C.G. and Williams, J.C. (1978). In: Toughness and Fracture Behavior of Titanium, STP 651, pp. 115-153, ASTM, West Conshohocken, PA. 13. Williams, J.C., Froes, F.H., Chesnutt, J.C., Rhodes, C.G. and Berryman, R.G. (1978). In: Toughness and Fracture Behavior of Titanium, STP 651, pp. 64-114, ASTM, West Conshohocken, PA. 14. Terlinde, G.T., Duerig, T.W. and Williams, J.C. (1983) Metall. Trans. A 14A, 2101. 15. Terlinde, G.T. and Schwalbe K.-H. (1987). In: Microstructure, Fracture Toughness and Fatigue Crack Growth in Titanium Alloys, pp. 97-109, Chakrabarti, A.K. and Chesnutt, J.C. (Eds.). TMS, Warrendale, PA. 16. Terlinde, G.T., Rathjen, H.-J. and Schwalbe K.-H. (1988) Metall. Trans. A 19A, 1037. 17. Haynes, M.J. and Gangloff, R.P. (1998) Metall. Trans. A 29A, 1599. 18. Young, G.A. and Scully, J.R. (1994) Corrosion 50, 919. 19. Gaudett, M.A. and Scully, J.R. (1999) Metall. Trans. A 30A, 65. 20. Gaudett, M.A. and Scully, J.R. (2000) Metall. Trans. A 31A, 81. 21. Nelson, H.G. (1992). NASP Government Work Package #92, NASA Ames Research Center, Moffett Field, CA. 22. Somerday, B.P. and Gangloff, R.P. (1998) Matls. Sci. Engr. A A254, 166. 23. Somerday, B.P. and Gangloff, R.P. (1998) Matls. Sci. Engr. A A254, 179. 24. Young, L.M., Young, G.A., Scully, J.R. and Gangloff, R.P. (1995) Metall. Trans. A 26A, 1257. 25. Somerday, B.P., Young, L.M. and Gangloff, R.P. (2000) Fatg. Fract. Engr. Matls. Struct. 23, 39. 26. Kolman, D.G. and Scully, J.R. (1998). In: Effects of the Environment on the Initiation of Crack Growth, ASTM STP 1298, pp. 61-73, Van der Sluys, W.A., Piascik, R.S. and Zawierucha, R. (Eds.). ASTM, West Conshohocken, PA. 27. Kolman, D.G. and Scully, J.R. (1997) Metall. Trans. A 28A, 2645. 28. Kolman, D.G. and Scully, J.R. (1999) Phil. Mag. A 79, 2313. 29. Kolman, D.G., Gaudett, M.A. and Scully, J.R. (1998) J. Electrochem. Soc. 145, 1829. 30. Oriani, R.A. (1987) Corrosion 43, 390. 31. McMahon, C.J., Jr. (2001) Engr. Frac. Mech. 68, 773. 32. Gangloff, R.P. (2001). “Diffusion Control of Hydrogen Environment Embrittlement in High Strength Alloys”, In: Hydrogen Effects on Material Behavior, Moody, N.R. et al. (Eds.). TMS, Warrendale, PA, in review. 33. Robertson, I.M. (2001) Engr. Frac. Mech. 68, 671. 34. Nelson, H.G. (1973) Metall. Trans. A 4, 364. 35. Scully, J.R. (2000). In: Environmentally Assisted Cracking, STP 1401, pp. 40-69, Kane, R.D. (Ed.). ASTM, West Conshohocken, PA. 36. Somerday, B.P., Wilson, A.W., Howe, J.M. and Gangloff, R.P. (2001) ”Microstructural Cause of Intergranular Hydrogen Environment Embrittlement of Aged Beta-Ti Alloys”, Metall. Trans. A, in review. 37. Graham, D.E. and Koss, D.A. (1978) Metall. Trans. A 9A, 1435.
RkJQdWJsaXNoZXIy MjM0NDE=