ICF10B

Therefore, it was imperative to include oxidation in the dynamic crack model in addition to the nonlinear fiber creep. However, additional modeling remains and more experimentation is planned. Crack growth appears to be controlled by FR above the composite matrix-cracking threshold at elevated temperatures in inert environments. PNNL and others have determined composite deformation rates[1,2,2435] and activation energies under these conditions and they match quite well with activation energies for fiber creep, about 500 – 600 kJ/mol. Our dynamic crack growth model agrees reasonably well with measured crack growth rates and these activation energies. When oxygen is introduced during the crack growth testing the deformation rates increase and the activation energy decreases to about 50 kJ/mol, in agreement with carbon oxidation processes. Significantly, the crack growth kinetics change from nonlinear to linear since now the bridge compliance is dominated by the linear portion as lfree + lox approach and exceed ldeb. Again, our model agrees well with these changes in both kinetics and activation energies. The transition between the FR and IR mechanisms is defined as the locus of points where the crack growth rates of each mechanism are roughly equal. This was determined by choosing an oxygen concentration where the crack velocity doubled compared to the velocity without any oxygen. This curve is steep as shown in Fig. 2 due in part to the high activation energy of the fiber creep process. It is bounded at high temperatures by fiber stress rupture mechanisms. Transitions from IR to either OE or VS/OE mechanisms are shown. We find that there is a competition between specimen failure due to IR relative to the time for pinch-off and OE to occur. The dynamics are handled by removing those fibers from the bridging zone that have an oxide thickness greater than some critical value, such as the interphase thickness. However, this transition is crack length (specimen size) and interphase thickness dependent. The size effect occurs since OE depends on total fiber exposure time, which is dependent on crack length. Interphase thickness effects arise due to our criterion that pinch-off occurs prior to the onset of OE. The computations shown here are for an interphase thickness of 150 nm. Other plausible OE mechanisms only require a critical oxide thickness that is not interphase thickness dependent [36,37]. However, such mechanisms will still exhibit a specimen size effect or history effect. Transitions from OE (pinch-off with brittle glass phase) to VS/OE (non-brittle, viscous glass phase) depend on the viscosity of the glass which is strongly dependent on glass composition. Thus, these transitions are not rigorously defined here and will have to wait for future work. By incorporating existing models of viscous interphase mechanics, we will be able to understand the effects of viscosity on fiber stress concentrations. The database for fiber stress rupture is mainly limited to tests in air so dependence on oxygen concentration is lacking. SR competes with OE and IR at temperatures higher than about 1373K for oxygen concentrations near 0.2 The onset of SR occurs at 1373K in air during dynamic crack growth according to our model and this onset is predicted to shift to 1423K for lower oxygen concentrations. Without detailed data as a function of oxygen concentration, we cannot be more quantitative. The map suggests that SR shifts to higher temperatures as the oxygen concentration decreases. The boundary between FR and SR is suggested to occur at the fiber thermal limits. There is a need for additional stress rupture data as a function of oxygen concentration. SUMMARY We developed a dynamic crack-growth model with the following features: 1) it is based on the weightfunction method using discrete fiber bridges, 2) it contains nonlinear bridge extension laws based on fibercreep kinetics for Nicalon-CG and Hi-Nicalon fibers, 3) it contains bridge extension laws for the case of interphase removal, and 4) it provides fully dynamic crack tracking using a critical-stress-intensity propagation criterion. The model reproduces the time-dependent crack-growth kinetics observed

RkJQdWJsaXNoZXIy MjM0NDE=