ICF10B

Evaluation of High-cycle Fatigue Life of Aluminum Cast Alloy from Meso-level Consideration Hiroshi NOGUCHI 1 and Tatsujiro MIYAZAKI 2 1Department of Mechanical Science and Engineering, Faculty of Engneering, Kyushu University, 6-10-1 Hakozaki, Fukuoka 812-8581, JAPAN. 2Graduate School of Engneering, Kyushu University, 6-10-1 Hakozaki, Fukuoka 812-8581, JAPAN. ABSTRACT In this paper, a growth rate law of a small crack under a large scale yielding is proposed for a generic metal material. A method is also proposed for considering the size distribution of spheroidal defects which interest with the specimen surface. Both methods are used to predict the high-cycle fatigue life with the large scatter due to the presence of defects. Moreover, rotating bending fatigue tests are carried out on Aluminum Cast Alloy with eutectic Si, Fe compounds and porosities. The present method for predicting fatigue life reliability from the meso-level consideration is examined and confirmed by comparing the predicted fatigue life distribution. KEYWORDS Metal Fatigue, Aluminum Cast Alloy, Fatigue Life, Fatigue Crack Growth, Statistics, Defect, Porosity, Recycle INTRODUCTION From a necessity of light transportation machine with a high specific strength, Aluminum Cast Alloy has been used in the engine and so on. 80% of material fracture is due to the fatigue. Therefore it is important to evaluate the fatigue characteristics as mechanical properties for machine designs. Moreover the results are useful for the improvement of reliability and alloy design. In researches on aluminum cast alloy, although many researches especially on shape and quantity of eutectic Si have been carried out [1-6], there are few researches on the effect of Fe introduced during the recycling process [2,3]. Fe forms a coarse needle shaped metal compound, and the compound decreases the flow of the melts and the mechanical properties. In order to decrease the bad effect of Fe, transition metals (Mn,Cr,Be and so on) are added to the aluminum cast alloy to improve the fracture toughness and breaking elongation by changing the Fe-compound’s structure from a needle type to a Chinese script type [8-11]. The changing ratio depends on the composition ratio of the transition metal to Fe [12] and amount of an improving element Sr [13,14]. It is necessary to evaluate the effect the various Fe-compounds on the fatigue characteristics simply and quickly. As afore mentioned, although it is necessary for practical use of new materials to evaluate the fatigue characteristics, a traditional macro-scale materials testing is useless because of the required long testing time. In order to overcome the problem, a new evaluation system for fatigue characteristics is constructed in this paper from meso-level considerations. Then it becomes possible to evaluate the fatigue characteristics of practical structures rapidly and to point out the direction of the material design reasonably. PREDICTION OF HIGH CYCLE FATIGUE LIFE In this paper, the high-cycle fatigue life characteristics are divided into the fatigue crack growth characteristics and the maximum defect size. Versatile fatigue crack growth law (stress ratio=−1) Under a small scale yielding condition, for example σa <0.5σS [15,16], the fatigue crack growth rate d`/dN , where ` is the total crack length on the specimen surface and N is a number of stress repetitions, is expressed as a the power of the stress intensity factor range, ∆K, as follows. d` dN =C(∆K)m (1) Here, σa is the stress amplitude, σS the yield stress, ` the total crack length on the specimen surface and N a number of cycle. On the other hand, under a large scale yielding condition, for example σa >0.6σS [15,16],

RkJQdWJsaXNoZXIy MjM0NDE=