ICF10B

In this study, thermal fatigue of a tool during die casting of aluminium and brass was experimentally evaluated. A selection of surface treatments and PVD coatings of a reference hot work tool steel were included. The following conclusions can be drawn. • Through induction heating the test equipment makes it possible to simulate failure of surface engineered tools during thermal cycling, as well as to deduce the surface strains responsible for the failure. • Thermal fatigue cracking of a surface engineered tool steel is influenced by the modification of the mechanical properties of the substrate which occurs during the engineering process. • With the exception of duplex-treatment, all variants of surface engineering show a tendency to decrease the resistance to thermal fatigue cracking as compared to the reference steel. However, the fact that the duplex-treated PVD CrN coating increased the resistance to thermal fatigue cracking as well as reduces the density of cracks as compared to the single-layered CrN coating, the potential to improve the life and performance in for example die casting applications still prevails. • The initiation and progress of the crack network in CrN coatings on top of tool steel has been described. • It is clearly demonstrated that the crack growth rate is rapidly increasing with the maximum cycle temperature above 700 °C. This indicates that an attempt to increase the life of tools exposed to thermal cycling should aim at decreasing the maximum temperature. ACKNOWLEDGEMENTS The financial and material support by the KK-foundation, Uddeholm Tooling AB, TA Hydronics AB and Bodycote Värmebehandling AB are hereby acknowledged. Special thanks to research engineer Anna Persson for all help with specimen preparation prior to light optical microscopy. REFERENCES 1. Sully, L.J.D. (1988). In: Metals handbook, Vol. 15, pp. 286-295, ASM International, USA. 2. Davis, J.R. (ed.) (1995). ASM speciality handbook, Tool materials, ASM International, USA. 3. Allsop, D.F. and Kennedy, D. (1983). Pressure diecasting, Part 2: The technology of the casting and the die, Pergamon Press Ltd, Oxford. 4. Kovrigin, V.A., Starokozhev, B.S. and Yurasov, S.A. (1980) Met. Sci. Heat Treat. 22, 688. 5. Danzer, R., Sturm, F., Schindler, A. and Zleppnig, W. (1983) Gisserei-Praxis. 19/20, 287. 6. Zleppnig, W., Danzer, R., Fischer, F.D. and Maurer, K.L. (1986) Proc. Euro. Conf. on Fract. 6, 1139. 7. Schindler, A.M. and Danzer, R.B (1989) Proc. Int. Conf. Step into the 90’s. 3, 905. 8. Chellapilla, S., Shivpuri, R. and Balasubramaniam, S. (1997) Trans. 19th Int. Die Cast. Congr. Exp. 295. 9. Arai, T. (1995) Trans. 18th Int. Die Casting Congr. Exp. 327. 10. Mitterer, C., Holler, F., Ustel, F. and Heim, D. (2000) Surf. Coat. Technol. 125, 233. 11. Starling, C.M.D. and Branco, J.R.T. (1997) Thin Solid Films. 308-309,436. 12. Wang, Y. (1997) Surf. Coat. Technol. 94-95, 60. 13. Faccoli, M., La Vecchia, G.M., Roberti, R., Molinari, A. and Pellizzari, M. (2000) Int. J. Mat. Prod. Technol. 15, 49. 14. Persson, A. (2000). Licentiate Thesis, Department of Materials Science, Uppsala University. 15. Sehitoglu, H. (1996). In: ASM handbook, Vol. 19, pp. 527-556, ASM International. 16. Suresh, S. (1998). Fatigue of materials, Cambridge University Press, UK.

RkJQdWJsaXNoZXIy MjM0NDE=