ORAL/POSTER REFERENCE: ICF100237 EXPERIMENTAL RESEARCH ON FRACTURE AND FATIGUE OF SCT SPECIMEN SIMULATING HIGH-STRAIN REGION OF PRESSURE VESSEL NOZZLES Chen Xuedong Yang Tiecheng Cheng Chuanqing Hefei General Machinery Research Institute No.888, West Changjiang Road, Hefei 230031, China Jiang Jialing Zhejiang University ABSTRACT This paper makes an in-depth analysis and research on the shaped compact tensile specimen (SCT), which simulates the high strain zone of pressure vessel nozzle. The elastoplastic FE analysis and test of SCT specimen show that SCT specimen fully possesses the characteristics of stress and strain simulation of high strain zone of pressure vessel nozzle, which is able to realize simulation of high strain zone of engineered structure with small test specimen and can conveniently change stress-strain field of the test specimen through changing the scale of geometric dimension, open size and shape of the test specimen. The rotational factor and crack tip opening displacement of SCT specimen are measured, The influence of local high strain plastic zone and the closing effect of the structure on fatigue crack propagation rate is studied and the engineering calculation method for COD of high strain zone and propagation rate of fatigue crack is proposed through theoretical analysis and calculation of fracture fatigue parameters of SCT specimen and experimental research and analysis of fracture fatigue crack propagation of SCT specimen, which provides a basis for fracture and fatigue assessment of high strain zone of pressure vessel nozzle. KEYWORDS pressure vessel, nozzle, high strain zone, SCT specimen, fracture, fatigue crack propagation 1. INTRODUCTION High-strain zone of pressure vessel nozzle yields higher stress concentration due to continuous destruction of geometric structure, resulting in very high stress-strain level within local region. Meanwhile, complicated structure of nozzle location increases the degree of difficulty of fabrication inspection, therefore, occurrence of welding defects can not be thoroughly avoided. Moreover, the effect of welding residual stress and performance deterioration of material adjacent to welds make this location extremely susceptible to fracture and fatigue damage of pressure vessel[1]. In recent 30 years, many countries launched extensive research on the subject of fracture fatigue in pressure vessel nozzle. Man has been seeking medium and small-sized specimens that can simulate the characteristics of the nozzle location of the real-sized vessels for effective fracture fatigue analysis[2], models such as wide plate, flat-plate nozzle, shaped plate, shaped CT specimen(SCT), bi-directional loading cross shaped plate etc. Research results[3] show that SCT specimen has the advantage of compact structure, small test load etc, which provides a more effective way for fracture and fatigue research of high-strain zone of pressure vessel nozzle. 1 In this paper the plastic rotational factor and COD of SCT specimen are measured, the effect of local high-strain plastic zone and closing effect of the structure on propagation rate of fatigue cracks is researched and the engineering calculation method for COD and propagation rate of fatigue cracks of high-strain zone is proposed through theoretical analysis and calculation of fracture fatigue parameters of SCT specimen and experimental research and analysis on fracture and fatigue crack propagation of SCT specimen in combination with FE stress-strain analysis and test stress measurement of SCT specimen, thus providing a basis for fracture and fatigue assessment of high-strain zone of pressure vessel nozzle.
RkJQdWJsaXNoZXIy MjM0NDE=