Tε * = ∆T ε * N∑ (2a) where ∆T= ∆Wn1 −(ti +∆ti ) ∂∆ui ∂x1 −∆ti ∂ui ∂x1 Γε ∫ dΓ (2b) (2b) The current T*ε, as defined by Equation (2), is thus dependent on the prior loading history, a property that is essential for elasticplastic analysis under crack growth. Although such incremental analysis can be routinely conducted by finite element analysis, it is not practical in experimental analysis as the cumulative experimental errors per load step will eventually overwhelm the sought data. Fortunately, Pyo et al [4] have shown, through numerical experiments, that the total T*ε integral computed directly by using the stresses and strains based on the incremental theory of plasticity, was for practical purpose equal to the summed ∆T*ε of Equation (2). Thus Equation (1) can be used for crack growth study without the cumbersome incremental procedure provided the states of stress and strain are based on the incremental theory of plasticity. More recently, T*ε was also studied extensively by by Nishioka and his colleagues [5]. ε is governed by the plate thickness for a plane stress state to exist along the integration contour of Γε. This distance, ε, is equated to the plate thickness after Narashimhan and Rosakis [6]1. For a plane strain state, this characteristic distance could be several times the crack tip radius. METHOD OF APPROACH By restricting the integration contour very close to and along the extending crack, Okada and Atluri [7] have shown that the contour integration trailing the crack tip can be neglected by virtue of the closeness of Γε to the traction free crack surface. Since the contour integral is now restricted to the frontal portion of Γε , the deformation theory of plasticity can now be used to compute the stresses in the loaded portion of Γε. The experimental procedure consisted of measuring the two orthogonal displacement fields surrounding a stably growing or a rapidly propagating crack in thin, single edge notched (SEN), central notched (CN) and compact (CT), 2024-T3 aluminum specimens. The strains and stresses, using the equivalent stress-strain and the measured uniaxial stress-strain data of the 2024-T3 sheet, were computed. Finally, Equation (1) was evaluated numerically along the contour, Γ ε . RESULTS SEN and CN Specimens Experimentally determined T*ε integral data of one SEN specimen and five CN specimens of different cracks lengths with saw cut or fatigued crack tip are shown in Fig. 1. For a contour size of Γε = 1 mm, the T*ε data for the 152.4 mm and 254 mm wide specimens are approximately equal. Other than the 50.8 mm wide CN specimens, the experimental T*ε data of the SEN and CN specimens practically coincide thus suggesting that the T*ε is a geometry-independent material property of this material. The T*ε resistance curve represents the average of this data. As shown in Fig. 1, the T*ε resistance curve rises at the initial stage of crack growth and reaches a constant value during steady crack growth. In contrast, the global J resistance curve, JR, continually rises with stable crack extension and includes energy from other sources. Al 2024-T3 T* Resistance Curves t=0.8mm, Γ ε =1mm, Tstarcur.spw Crack Extension (mm) 0 2 4 6 8 10 1 T*ε Integral (MPa mm) 0 20 40 60 80 100 120 140 160 SEN - Exp (W=25.4mm, a=6.4mm) CN - Exp (W=50.8mm, 2a=12.7mm) CN - Exp (W=50.8mm, 2a=12.7mm) CN - Exp (W=152.4mm, 2a=50.8mm) CN - Exp (W=254mm, 2a=114.3mm) CN - Exp (W=254mm, 2a=114.3mm) SEN - FE CN (W=50.8mm) - FE CN (W=254mm) -FE T*ε Resistance (Ave) 2 1 The three-dimensional elastic-plastic finite element analysis of a flat crack in plate by Narashimhan and Rosakis [17] showed that the plane stress state prevailed at one half of the plate thickness from the crack tip. Since a 100 percent shear lip is the norm in ductile fracture, the minimum distance, ε, was conservatively picked as the plate thickness.
RkJQdWJsaXNoZXIy MjM0NDE=