ICF10B

Fig. 1. SEN and CN experimental T*ε resistance curve ( Γε = 1mm) While the J integral based instability criterion is determined on a global basis, the instability criterion for T*ε integral is locally based. During steady crack growth, the state of stress is in equilibrium and thus the parameter characterizing this phenomenon should be constant. When the driving force exceed the material’s resistance, i.e. T*ε > T*εR., instability will occur without an additional applied load or a displacement. For crack growth simulation, a load or displacement was applied as the boundary condition and the crack was propagated when T*ε > T*εR. With the prescribed load or displacement held constant, T*ε was evaluated again for the extended crack. If T*ε remained greater than T*εR , the crack was extended again, and T*ε was re-evaluated. The crack continued to extend until T*ε dropped below T*εR. Additional load/displacement was applied to the specimen until T*ε was equal to T*εR where upon another node was released to extend the crack. This procedure was repeated until no additional load or displacement was required to propagate the crack. At that point, instability was assumed to have occurred. The results identified as “FE” in Fig. 1 show that this simulation compared very well with the experimental data. Curved Crack Growth Twenty four biaxial test specimens were fabricated without or with bonded, bonded and riveted and integral pad-up tear straps and tested to failure. The results obtained in six tests, i.e. without tear straps, with bonded, bonded and riveted and machined pad-up tear straps are report in this paper. Figure 2 shows the variation in T*1 ε, which corresponds to the mode I contour integral of Equation (1), along the frontal portion of Γε at various crack tip locations of the curved cracks. The steady state T*1 ε in this study coincides with the corresponding T*ε resistance curve of Fig. 1. The increase in T*1 ε of Experiments B21 and B25, as the crack Fig. 2. T*1 ε variation with curved crack growth. approaches the tear strap, represents the increased resistance to crack growth in these machined pad-up tear straps. Such an increase was not observed in Experiments B9 and B15, thus suggesting that the bonded and bonded-riveted tear straps may not be as effective as the machined pad-up tear straps in resisting curve crack extension. Indeed, the final load at fracture in the machined pad-up tear straps was 30 percent higher than that of the bonded and bonded-riveted tear straps. T*2 ε, which is the mode II equivalent of T*1 ε, oscillated about its null value throughout the entire curved crack extension. These results suggest that T*1 ε is the resistance for a locally self-similar crack growth and that the crack curves in the direction of vanishing T*2 ε. These results are the elastic-plastic counterpart to the vanishing KII criterion for curved elastic crack growth [8,9]. The experimentally determined value of T*1 ε during stable crack growth is approximately 120 MPa-mm which is 5 percent higher than the T*! ε resistance curve in Figure 1. Crack Link-up The feasibility of using the T*ε resistance curve of Fig. 1 to predict crack growth and linkup in the presence of mulitple site damage (MSD) was tested through a series of MSD experiments. The experimental procedure consisted of determining the T*ε integral experimentally and measuring the crack growth and linkup in MSD2 specimens with two cracks, MSD3 specimens with a center/lead crack approaching two holes with MSD cracks and MSD5 specimens with a center/lead crack and four holes. These specimens were machined from the same Al 2024-T3 clad aluminum sheet of thickness 0.8 mm. All cracks were oriented in the LT direction and special buckling guides were used to prevent the out-of-pane buckling of the fracture specimen. Specimens MSD5_08 (ligament = 12.7 mm and amsd = 2.5 mm) and MSD5_13 (ligament 20.32 mm amsd = 2.5 mm) failed simultaneously with the first crack linkup. The experimental T*ε versus crack extension for both specimens are shown in Figs. 3(a) and (b). In both cases, all the cracks exhibited stable crack growth at T*ε values similar to the CN specimen. Crack tips C and

RkJQdWJsaXNoZXIy MjM0NDE=