ORAL/POSTER REFFERENCE: ICF100986OR FATIGUE AND HYDROGEN CRACKING IN CANNONS WITH MECHANICAL AND THERMAL RESIDUAL STRESSES J. H. Underwood1, A. P. Parker2, E. Troiano1, G. N. Vigilante1, M. D. Witherell1 1Army Armament Research, Development and Engineering Center, Watervliet, NY 12189 USA 2Royal Military College of Science, Cranfield University, Swindon SN6 8LA UK ABSTRACT Bauschinger-modified autofrettage residual stresses are used to improve the fatigue intensity factor model for fatigue life of cannon pressure vessels. Effects of yield strength and initial crack size are included with applied and residual stress in a S-N description of cannon tube life that matches full-scale cannon fatigue test results with a R2 correlation of 0.92. Thermally induced residual stress near the bore of a fired cannon is modeled by finite difference calculations of temperature and mechanics calculations of transient thermal stress and resulting residual stress. Temperature dependent thermal and physical properties are used, and the temperature distributions are validated by direct comparison with the known temperatures and the observed depths of microstructural damage and transformation in fired cannons. Calculations of fatigue life and yield pressure for a range of applied pressure, diameter ratio, yield strength and % autofrettage agree well with measurements from full-scale cannons. Increased life is predicted for increases in yield strength and % autofrettage, although the Bauschinger effect significantly reduces the amount of life increase for autofrettage above 50%. The combined effects of mechanically induced residual stress and thermally induced residual stress on cannon fatigue life are calculated, using an increased initial crack size to account for thermal residual stress. Calculations of fatigue life are presented for a range of applied pressure and for selected gas temperatures. KEY WORDS: metal fatigue, pressure vessels, autofrettage, thermal stress, high strength steels, hydrogen crack INTRODUCTION The benefit of mechanically induced autofrettage residual stress in extending the fatigue life of a pressure vessel has been known for decades. Only relatively recently has comprehensive predictive analysis of autofrettage residual stress been available that can account for the actual material properties of pressure vessel steels, most importantly the significant reduction of compressive yield strength that occurs in an autofrettaged vessel, known as the Bauschinger effect. Measurements of the Bauschinger effect in the Ni-Cr-Mo steels commonly used in cannon pressure vessels have long been available [1]. Analysis of the Bauschinger strength reductions that are observed for different vessel diameter ratios and degrees of autofrettage was described by Chaaban et al [2], but they used a simple bilinear representation of the reduced compressive yielding, whereas a much more complex non-linear behavior is observed. Parker [3] has provided useful expressions that will be used here to calculate autofrettage residual stresses at the bore of pressure vessels with Ni-Cr-Mo type Bauschinger properties, accounting for diameter ratio, degree of autofrettage and non-linear behavior, the effects of concern here. In the past decade a troublesome type of thermally induced residual stress has been found to affect cracking and service life of cannon pressure vessels. Underwood et al [4] showed metallographic evidence of a constantdepth array of cracks at the inner surface of fired cannon tubes that cannot be explained by a mechanical fatigue process. Finite difference calculations of the transient temperatures at the inner surface of a fired cannon tube predicted yield-level transient compressive stresses to about the same depth as the crack array, suggesting that tensile residual stress was present to this depth. Given that significant hydrogen is produced in cannon firing and cannon steels are highly susceptible to hydrogen cracking, the constant-depth cracks can be explained as
RkJQdWJsaXNoZXIy MjM0NDE=