hydrogen cracks. In the work here additional finite difference temperature calculations and transient and residual stress calculations are performed, to determine the effect of thermally induced residual stresses and cracking on fatigue life of cannon pressure vessels. The fatigue life implications of both the mechanically induced autofrettage residual stresses and the thermally induced firing residual stresses will be described in the work here using the fatigue intensity factor (FIF) concept developed by Underwood and Parker [5]. This modified S-N approach gives a high correlation, single-expression description of fatigue life for a wide range of vessel configuration, stress concentration, applied and residual stresses, yield strength and initial crack size. ANALYSIS The residual stresses in a cannon pressure vessel that will be discussed here are those produced by a mechanical mandrel-swage autofrettage process during fabrication of the cannon tube and those produced by the transient convective heating of the inner surface (ID) of the tube during cannon firing. Transient heating of a cannon ID during firing has traditionally been important only because it would initiate fatigue cracking somewhat earlier than would otherwise be expected. However, with increases in cannon firing pressures, temperatures and duration, ID thermal damage is deeper and asserts a more significant control over cannon fatigue life than in the past. The finite difference method is used to calculate the near-ID transient temperature distribution, as the initial measure of the degree and depth of thermal damage. The temperatures are then used to calculate the biaxial transient compressive stresses and the tensile residual stresses in the locations of the steel substrate where the compressive stresses exceed the yield strength. The depth of a significant tensile residual stress is taken as the important final measure of thermal firing damage, because hydrogen cracking is expected to occur to this depth in the steel and thereby accelerate the fatigue failure process. Autofrettage Residual Stresses and Yielding The familiar Tresca-plane stress expressions for hoop residual stress in an autofrettaged tube were modified [3] to apply to the Mises-open end conditions that are more appropriate for cannon pressure vessels and also to include the effect of the Bauschinger reduced strength. These modified expressions are: SθR = RS [ -pY + SY [1+ ln(r/a)] - pY a 2(b2-a2) (1+b2/r2) ] for: a < r <r Y [1] pY = RP [ SY [ln(rY/a) + (b 2- r Y 2)/2b2] ] [2] where a and b are the inner and outer tube radii, rY is the autofrettage radius, SY is yield strength, pY is the equivalent pressure that would be required to accomplish the mandrel autofrettage, and RS and RP are the ratios that accomplish the modification for various degrees of autofrettage, n. At the critical ID, i.e., at r = a: RS = 1.669 – 0.165(b/a) – 0.730 n 3 +1.984 n2 – 1.887 n for: 1.75 < b/a < 3.00; 30% < n < 80% [3] RP = 1.155 / [ 1+ 1 / 3(b/a) 4 – 2.3 n]1/2 for: n < 70% [4] Equations 1-4 are used here to calculate the mechanically induced hoop residual stresses at the ID of autofrettaged tubes, including the important effect of the Bauschinger reduced strength for the type of Ni-Cr-Mo steels used in cannons. Once the Bauschinger-modified hoop residual stresses are known, the Bauschingeraffected pressure, p*, at which the cannon tube re-yields when re-pressurized following initial autofrettage can be determined, using the Mises criterion in the notation here: SY = [ [(SθT – p*) 2 + (p* - ν SθR) 2 + (ν SθR - SθT) 2] / 21/2 ]1/2 for r = a [5] where SθT is total hoop stress (sum of applied and residual) and ν SθR is an estimate of axial residual stress [3]. Equation 5 gives a Bauschinger-modified ID yield pressure, but it does not include any effect of additional reyielding discussed by Parker [3] that can occur near the yield pressure. This will be considered in future work. Transient Temperatures and Thermal Residual Stresses Finite difference calculations of one-dimensional convective heat flow were used to determine the near-ID temperatures produced by cannon firing conditions. The calculations used increments of 0.02 mm in depth below the heated bore surface. About fifty increments were required for the temperature to drop from typically
RkJQdWJsaXNoZXIy MjM0NDE=