below the bore surface, for the following input values: the δ and k properties for chromium and steel from Table 1; Tgas = 2160 K and 0.008 s pulse duration; and h = 193,000 W/m2 oK. Note that the depths and temperatures of the 1320 K and 1020 K transformations of chromium and steel are well matched for the calculated temperature distribution, so it should be a useful basis for transient and residual stress calculations. These stress calculations are shown in Fig. 2 for selected ranges of depth somewhat below the bore surface; calculations very near the bore surface have little meaning due to the lack of information on material properties at the temperatures in this region. The significant region of tensile residual stress up to about 0.38 mm below the bore surface is alarming, considering the presence of hydrogen and the susceptibility of high strength cannon steel to hydrogen cracking. Residual Stress Effects on Fatigue Life and Yielding Fatigue lives calculated using the FIF concept for typical cannon conditions are shown in Fig. 3 for a range of fatigue pressure and various autofrettage conditions. Yield pressures for the cannon tube calculated from Eq. 5 are also shown. The results for 0% autofrettage, with the drastically lower lives and yield pressure, show how critical the autofrettage process is for cannon pressure vessels and similar high strength steel vessels. The lives and yield pressures for 30%, 50% and 70% autofrettage include the Bauschinger effect (BE) and show increases for increased autofrettage, but noticeably smaller increases in life and yield pressure are evident for additional autofrettage above about 50%. This diminishing return is a direct consequence of the progressive decrease in effective yield strength in steel vessels that accompanies an increase in degree of autofrettage. When the Bauschinger effect is not included in the calculation of fatigue life, such as the dashed curve example in Fig. 3, the decrease in yield strength is not accounted for, and dangerously non-conservative calculations of fatigue life and yield pressure are produced. 500 600 700 800 900 1000 0 5,000 10,000 15,000 20,000 25,000 calculated fatigue life, Ncalc ; cycles fatigue pressure, MPa - calculated yield pressure 0% 30% 50% 70% autofrettaged; with BE autofrettaged 50%, noBE pY = 914 Mpa; 50%, no BE pY = 834 Mpa; 50%, with BE Sy = 1200 MPa; b/a = 2.00; ai = 0.10 mm Figure 3: Life and yield pressure for various % autofrettage Fatigue life and yield pressure calculations of a similar type to those of Fig. 3, but for actual cannon conditions, are shown in Fig. 4, typical of the chamber area of a tank cannon, with a b/a = 1.97, 60% autofrettage, and ai = 0.10 mm. In contrast to the diminishing effect of % autofrettage in Fig. 3, there is no diminishing effect of increases in yield strength on either life or yield pressure. For the same degree of autofrettage, and thus the same relative reduction in effective yield strength by the Bauschinger effect, increases in material yield strength are rewarded with significant increases in life and yield pressure (but at the expense of decreased resistance to fast and environmental cracking). Results from one of the groups of cannon fatigue tests described earlier are also shown in Fig. 4, plotted at the 670 MPa pressure used in the tests and the mean and range of fatigue life from the tests. These results provide a good verification of the methods of life calculation described in the work here, because the mean life from the tests falls very close to the correct position, just to the right of the SY = 1100 MPa curve, as would be expected for the 1120 MPa mean yield strength of the tests. The test results also show, by their close proximity to the yield pressure for SY = 1000 MPa, that the 670 MPa fatigue pressure for the tests was close to the yield pressure. 500 600 700 800 900 0 5,000 10,000 15,000 20,000 25,000 calculated fatigue life, Ncalc ; cycles fatigue pressure, MPa - calculated yield pressure Sy; MPa: 1000 1100 1200 1300 4 tests; b/a = 1.97 60 % autofrettage Sy = 1120 MPa Figure 4: Life and yield pressure for various yield strengths b/a = 1.97; 60% autofrettage; ai = 0.10 mm
RkJQdWJsaXNoZXIy MjM0NDE=