10000 100000 1000000 10000000 460 480 500 520 540 560 580 600 620 640 660 680 DP650+BH DP650 DP650 DP650+BH σ (MPa) N (cycles) Figure 5: S-N curves of 10% pre-strained DP650 with and without paint baking simulation TABLE 4 MECHANICAL PROPERTIES OF DP650 AND DP650+BH AFTER 10% PRE-STRAINING YS in MPa TS in MPa A80 in % ∆YS in MPa DP650 520 695 21 after pre-straining: 692-520=172 DP650+BH 836 837 6 after pre-straining and baking: 836-520=316 SUMMARY The investigated multiphase high strength steels show qualitatively better fatigue properties than the commercially used microalloyed grade. Their higher finite life range and especially their higher fatigue limit allow a lightweight design for many automotive applications as shown here for wheels, which are subjected to high fatigue requirements. The made assumptions concerning the effect of martensite and other phases as well as the effect of bake hardening on the fatigue behaviour of multiphase steels are still subject of investigation. Furthermore, the non-homogeneous loading sequences occurring in automotive structures during production and service have to be taken into account. REFERENCES [1] Theuwissen, J. (2000) Praktische toepassing van Slijtvaste Deklagen op Gereedschappen, internal report of the Ford wheel factory, Genk, Belgium [2] Ludwig, J. and Schulz-Forberg, B. (1994) Sicherheitsniveaus von Transporttanks für Gefahrgut. Bundesanstalt für Materialforschung und –prüfung. Research report 203, Berlin (Germany), p.41 [3] Girault, E., Jacques, P., Harlet, Ph., Mols, K., Van Humbeek, J., Aernoudt, E. and Delannay, F. (1998) Mater. Charact. 111, p.40 [4] Fuchs, H. O. and Stephens, R. J. (1980). Metal fatigue engineering. John Wiley, New York. [5] Vogt, J.B., Argillier, S., Leon, J., Massoud, J.P. and Prunier, V. (1999). ISIJ International 39, p. 1198 [6] Akdut, N. (1999) International Journal of Fatigue 21, S97 [7] In: Light-weight automotive construction with steel (1999) Technical Steel Research, Final Report, EUR 18412, Ed. and publisher: European Commission, Luxembourg, ISBN 92-828-5156-7, p. 222
RkJQdWJsaXNoZXIy MjM0NDE=