ICF10B

have been no data for fatigue crack growth properties which are important for actual MEMS devices. This is partly due to the lack of suitable fatigue testing machine for micro-sized materials. In our previous investigations, we have designed a new fatigue testing machine for micro-sized specimens [4, 5], and fatigue life curves have been obtained for micro-sized specimens prepared from a Ni-P amorphous alloy thin film [6]. Amorphous alloy thin films deposited on substrates by sputtering or plating techniques are considered to be potential candidate materials for MEMS devices because of their isotropic mechanical properties and high corrosion resistance. Therefore, it is important to clarify the fatigue crack growth properties of these amorphous thin films. However, the fatigue properties of micro-sized amorphous specimens have not yet been studied apart from our previous investigation on the fatigue life of a micro-sized Ni-P amorphous alloy specimens [6]. In this investigation, fatigue crack growth tests have been performed on micro-sized specimens prepared from an electroless deposited Ni-P amorphous alloy thin film and the size effects on the fatigue crack growth behavior of micro-sized specimens have been discussed. EXPERIMENTAL PROCEDURE Preparation of Specimens The material used in this investigation was a Ni-11.5 mass%P amorphous thin film electroless plated on an Al-4.5 mass%Mg alloy. The thickness of the amorphous layer was 12 µm and that of the Al-4.5 mass%Mg alloy substrate was 0.79 mm, respectively. A disk with a diameter of 3 mm was cut from the Ni-P/Al-Mg sheet by electro discharge machining. An amorphous layer was separated from the Al-Mg alloy substrate by dissolving the substrate with a NaOH aqueous solution. The amorphous thin film was fixed on a holder and two types of micro-cantilever beam specimens with dimensions of 10 (B) x 12 (W) x 50 (L) µm3 and 30 (B) x 12 (W) x 50 (L) µm3 were cut from the amorphous layer by focused ion beam machining. Figures 1 (a) and (b) show the specimens prepared by the above procedures. Notches with a depth of 3 µm were introduced into the specimens by focused ion beam machining. This notch depth is equivalent to a/W = 0.25, where a is notch length and W is specimen width. The width of the notch was 0.5 µm, and the notch radius is thus deduced to be 0.25 µm. The notch position was 10 µm away from the fixed end of the specimen. The loading position is set at 40 µm from the fixed end of the specimen. Fatigue Crack Growth Test Fatigue crack growth tests were performed in air at room temperature using the fatigue testing machine for micro-sized specimens. Fatigue tests were carried out at a frequency of 10 Hz and different stress ratios, R (R = Pmin / Pmax, where Pmin is the minimum load and Pmax is the maximum load applied over the fatigue cycle) of 0.1, 0.3, 0.5 and 0.7 under constant load amplitude (∆P/2, where ∆P = Pmax - Pmin) of 2 mN. This fatigue test condition was determined from our preliminary experiments. Although the crack length was not able to be measured directly in this testing machine, the change in specimen compliance 40µm 10µm 20µm B=10µm Loading W=12µm (a) (b) 20µm B=30µm Loading Figure 1: Two types of micro-sized cantilever beam specimens with different breadth (B) prepared by focused ion beam machining. (a) B=10mm and (b) B=30mm.

RkJQdWJsaXNoZXIy MjM0NDE=