ICF10B

predictive methods in the area of fatigue durability has resulted in over-conservative designs that often mitigate the advantages of using PMCs in primary components. To address these issues, an experimental investigation was made of the fatigue damage progression and damage tolerance of a 5-harness satin carbon fiber reinforced epoxy composite, AS4/PR500, subjected to fully reversed cyclic loading. Two datasets were created and examined. The first is the baseline data for the material behavior without environmental conditioning, i.e., 0 hrs. The second dataset consisted of material that underwent 12,000 hrs (12k hrs) of hygrothermal cycle (HC) conditioning. The elevated temperature fatigue behavior and damage progression was tracked through the measurement of the real-time tensile and compressive modulus. One unique feature of the work was to quantify the severity of fatigue damage via residual compressive strength measurements made at various degrees of actual compressive modulus degradation. Specifically, samples were subjected to residual compressive strength tests at approximately 0, 2.5, 5, and 7.5 % reductions of their initial compressive modulus. These data illustrate a relationship between fatigue damage progression as measured by the material’s effective modulus and the material’s damage tolerance while avoiding all assumptions with respect to the percentage of cyclic life. This detailed examination was completed on material from both datasets and then the data trends were compared. MATERIAL AND EXPERIMENTAL DETAILS All material was fabricated by a resin transfer molding (RTM) process at Dow U.T. (USA) from a single batch of resin and fiber mat into thick laminates (16 ply, 6.1 mm) with panel dimensions of 63.5 x 63.5 cm. Test coupons were machined using a diamond wheel grinding process. The HC conditioning, illustrated in Fig 1, was a nominal 85/30 (85 % relative humidity at 30 °C) exposure combined with a daily “mission cycle” consisting of a 90 minute exposure at 121 °C in a forced air convection oven. The cycle was selected as representative of a static component in the propulsor region of a gas turbine engine. The 12 khr conditioning was conducted on the material in large panel form prior to cutting the test coupons to avoid edge effects influencing the mechanical properties. The weight gain, shown in Fig. 2, was monitored using a traveler panel with a width to thickness ratio of 25 to 1. Note that the 90 min cycle at 121 °C was sufficient to prevent the material from reaching a moisture equilibrium state, even after 12k hrs. After conditioning and machining of the coupons, all material was vacuum dried for 48 hrs at 105 °C and stored in a dessicator until immediately prior to testing. Mechanical testing was performed on a computer controlled servohydraulic test frame. A radiant mini-furnace was used for specimen heating and strains were measured using edge-mounted extensometers with a 12.7 mm gage length. All mechanical testing was performed at 121 °C in a laboratory air environment. Time, hours 0 1 2 23 24 Temperature, °C 20 40 60 80 100 120 140 Relative Humidity, % 0 Temperature Relative Humidity oven air 85 Time, hours 0 4000 8000 12000 Weight Change, % 0.00 0.05 0.10 0.15 0.20 Condition: 85 %RH/30 °C + 90 min at 121 °C (Mon-Fri) Fig. 1-Hygrothermal Cycle (HC) Fig. 2-Weight gain during HC conditioning.

RkJQdWJsaXNoZXIy MjM0NDE=