available in published papers for design purposes. Additionally, it has to be noted that still today, the MIL Handbook procedure does not provide any detailed procedure for designing composite material components to fatigue. Finally, the damage development in composite laminates under cyclic loading usually follows clear sequences in the development of the basic damage modes, such as matrix cracking, interlaminar delamination, fiber failure, fiber-matrix pull up, and no new mechanism of failure with respect to quasi-static loading is generated under fatigue. The presence of a large scatter in the representation of experimental measurement sometimes can be an indicator of low correlation between the dependent and independent variables. The possibility to better understand the effective composite material performance has been initially offered by Talreja [7] reformulating constant stress amplitude data in terms of imposed strain. In this paper, fatigue behavior of composite laminates is reviewed comparing material performance under constant stress and constant strain amplitude. This approach confirms the role of the effective applied maximum strain as a governing parameter for fatigue performance estimations. A major outcome is that strain can be actively, reliably and continuously controlled in composite components in service using embedded sensors. CONSTANT STRESS AMPLITUDE AND CONSTANT STRAIN AMPLITUDE FATIGUE FEATURES Fatigue testing for composite materials has been traditionally performed under constant stress amplitude loading condition following the same approach used for metals. When loaded, damage can occur in a composite laminate in the form of matrix cracking, fiber failure, interlaminar delamination and fibermatrix debonding. The sequence of appearance of these basic failure modes is controlled by the lowest strain to failure of the composite constituents. An interesting feature is that no new damage mechanism is introduced by fatigue with respect to the monotonic quasi-static loading. Each of these basic damage modes modifies the material constitutive response. However, transverse matrix cracking, that is the first damage mode to appear both under quasi static and fatigue loading, is the responsible of the major reduction of the material stiffness. Transverse matrix cracking density increases with the increasing of the imposed strain (stress) until saturation occurs, a situation usually described as characteristic damage state (CDS). According to this, damage in composite laminates has been addressed focusing the attention on the evolution of the matrix crack density with cycles. Even though the relation between the stiffness reduction due to a given crack density is well assessed, the damage kinetic evolution law with cycles still needs to be assessed. As previously stated, this job is made even more difficult due to the large experimental data scatter that arise from constant stress amplitude testing. Bonora and Newaz [6] investigated fatigue performance of a number of composite laminates, varying stacking sequences, constituents, etc. They found that during constant stress fatigue, cyclic strain amplitude increases as a result of damage that lower material stiffness plus an additional strain ratcheting due to the non complete closure of generated cracks, Figure 1 . Additional strain accumulation can be also induced by visco-plastic material behavior. If the dominating part of the total accumulated strain is the one due to damage, strain amplitude increases until CDS is reached. After this point, stress amplitude and strain amplitude will be both constant during cycling similar to metals under stabilized cycle loading conditions. Newaz and Bonora [7] have found that this correlation between stress and damage is inadequate to describe the material damage evolution process as the assumption of uniform stress on the net section is
RkJQdWJsaXNoZXIy MjM0NDE=