ICF10B

Recent studies [4,5] on the HCF properties of a Ti-6Al-4V blade alloy, where FOD was simulated using high-velocity impacts of steel shot on a flat surface, have focused on the definition of threshold conditions for crack initiation and growth on subsequent fatigue cycling. The mechanistic effect of FOD was considered in terms of (i) the possibility of forming microcracks in the damage zone, (ii) the stress concentration associated with the FOD-induced notches, (iii) microstructural damage from FOD-induced plastic deformation, and (iv) the localized presence of tensile residual hoop stresses in the vicinity of the impact site. Although all these factors play an important role, a pivotal effect of FOD in reducing fatigue life in Ti-6Al-4V appears to be the formation, at high impact velocities, of damage-induced microcracks; on subsequent cycling, these act as preferred sites for the initiation of fatigue cracks in the pile-up of material around the rim of the impact crater, depending upon the relative magnitude of the residual stresses in the vicinity of the impact. For high applied stress ranges, HCF failures initiate directly at the impact site, whereas at correspondingly low applied stresses ranges, they initiate in locations away from the impact site. In analyzing the high stress failures, it was found that FOD-initiated microcracks, together with the stress concentration of the indent, were the prime reasons that the HCF failures initiated at the FOD sites. The microcracks (some as small as 1 µm) grew at applied stress intensities as low as ∆K = 1 MPa√m, which is well below the “worst-case” ∆KTH threshold in bi-modal Ti-6Al-4V [6] of 1.9 MPa√m for “continuum-sized” cracks, i.e., for cracks larger than the characteristic microstructural size-scales. Thus, although the “worstcase” threshold, which is determined at R → 1 to minimize crack closure, provides a critical lower-bound for the growth of HCF cracks in bi-modal Ti-6Al-4V, it only applies for “continuum-sized” cracks, which in this microstructure are larger than ~50-100 µm in length. Since the microcracks associated with impact damage are more than an order of magnitude smaller than this, an alternative approach is proposed to describe the threshold HCF conditions in the presence of FOD based on a Kitagawa-Takahashi diagram, where the limiting conditions for HCF are defined in terms of the stress concentration-corrected smooth-bar fatigue limit (at microstructurally-small cracks sizes) and the “worst-case” threshold (at larger, “continuum-sized” crack sizes). In contrast to HCF failures under high applied stresses, at low applied stress ranges failures were caused by fatigue cracks that initiated at locations remote from the impact site, specifically in regions of high tensile residual stresses. It is the purpose of this paper to examine the role of the relative magnitudes of the applied and residual stresses in dictating the sites for the initiation of HCF failures in impact-damaged Ti-6Al-4V, and to provide a methodology to describe the limiting threshold conditions for such failures at both low and high applied cyclic stresses. To achieve this objective, the residual stresses in the vicinity of the damage sites are computed numerically [7] and measured experimentally using synchrotron x-ray micro-diffraction. Such stresses are considered to affect the local load ratio for subsequent fatigue cracking, which is evaluated by determining smooth-bar stress-life (S-N) curves for load ratios from R = -1 to 0.8. Using such results, a modified Kitagawa-Takahashi approach is presented to provide a rational basis for the effect of FOD on HCF failures in Ti-6Al-4V at both high and low applied stresses. Additionally, we briefly consider the effect of laser shock peening (LSP) as a surface treatment to improve resistance to FOD-induced failures under HCF cycling [1,8]. In this study, the flat surfaces of fatigue samples were prepared by LSP processing prior to FOD event, and the subsequent fatigue lives compared to of samples without such surface treatment. EXPERIMENTAL PROCEDURES The Ti-6Al-4V alloy investigated, of composition (in wt.%) Ti-6.3Al-4.19V-0.19Fe-0.19O-0.013N-0.0041H, was from the forgings produced specifically for the U.S. Air Force National HCF Program. The bi-modal (solution treated and overaged) microstructure of this material, consists of ~60 vol.% primary α (grain size ~20 µm) within a lamellar α+β matrix. The alloy has yield and tensile strengths of 915 and 965 MPa, respectively, with a reduction in area of 45%, based on tests parallel to the length of the plate [4]. Foreign object damage was simulated by firing 1.0 mm or 3.2 mm diameter chrome-hardened steel spheres onto a flat specimen surface of tensile fatigue (so-called modified KB, details are given in Ref. [4]) specimens at an angle of 90º at velocities of 200 and 300 m/s using a compressed-gas gun facility. Impact velocities of 200 to 300 m/s represent typical in-service impact velocities on aircraft engine fan blades. The impact damage craters are also typical of those seen in service, with root radii similar to those of actual damage sites [2]. To evaluate the effect of surface treatments on the HCF resistance, the gauge and transition section of modified KB specimens were laser shock peened to induce compressive residual stresses to approximately 500 µm deep on each side. Following impacting with the steel spheres to simulate FOD, the damaged regions were examined in a highresolution, field-emission scanning electron microscope (SEM), prior to cycling at maximum stress values between 225 and 500 MPa at R = 0.1 and 0.5 (with a sinusoidal waveform).

RkJQdWJsaXNoZXIy MjM0NDE=