ICF10B

beam current. Almost of all the TiO2 thin films made by this method is confirmed that oxygen in the films decreased from surface in the depth direction, and the other element of Ti in the films increase from surface toward the depth direction. Chemical compositional depth profile obtained in this study showed that the crystal structure of TiO2 film obtained by using He ion beam had relative better crystallized structure. Then, the crystal structure of the coated TiO2 thin film was investigated by XRD and shown in Figure 4. From the result of crystal structure examined for thin films by X-ray Diffraction, no sharp peak strength was recognized both in Rutile structure and Anatase one. Therefore, the thin films obtained in this study by Ion-Beam-Mixing method showed relatively amorphous microstructure. However, in case when the TiO2 thin film was obtained using He ion for assisting comparatively crystallized microstructure of Rutile was obtained . Figure 4:TiO2 films diffraction pattern by XRD 30 40 50 60 0.5 1 1.5 il Assisted by Ar ion Assisted by n 2θ I(count)×10-3 Rut He io ● Rutile Natural Corrosion Potentials of TiO2 Thin Films in 0.3% NaCl Aqueous Solution Natural corrosion potentials of TiO2 thin coatings film were measured in 0.3% NaCl aqueous solution of 298K under the conditions of initial 2 hours without UV ray irradiation, next 2 hours with UV illumination and final 2 hours in dark again for both of Ar and He ions assisted films. In Figure 5 obtained results were indicated. From this figure, abrupt drop was recognized in the potential values when UV ray illumination was conducted. And then, gradual recover in the potential was recognized after UV ray was turned off. From these results, it was understood that the potentials gaps between UV ray illumination and dark were about 200mV and 120mV for He and Ar assisted TiO2 thin films, respectively. Therefor, it is confirmed that the shift of potential was generated in the negative direction. Therefore, TiO2 thin films showed the photo-catalytic function under UV ray illumination. Anodic Polarization Measurement of TiO2 Thin Films Coated Specimen in 0.3% NaCl Aqueous Solution The polarization curves of TiO2 thin films coated AISI 304 stainless steel specimen were obtained under UV ray illumination and non-illumination conditions in 0.3% NaCl aqueous solution of 298K and shown in Figure 6. Under UV ray illuminating condition both specimens made by Ar and He ions assisting showed no remarkable current density increase. In contrast, in case of non UV ray irradiated condition abrupt increase in the current density was recognized especially in He assisted TiO2 thin film and resulted in the pitting corrosion with local exfoliation of thin film. Therefore, TiO2 thin film has corrosion protecting performance under UV ray irradiating condition, even when TiO2 thin film has some inherent defect distribution in itself. Under dark condition, however, distributed inherent defects such as pinhole and so on played an important role in the localized corrosion process of TiO2 thin film coated SISI 304 stainless steel specimen. The adhesion strength between TiO2 thin film and substrate metal became relatively low especially in case when He ion assisted thin film in spite of having better photo-catalytic function. As a result, the pitting corrosion with local exfoliation was generated in this film. Cathodic Protection Performance of TiO2 Thin Film with Some Artificial Defect In the previous chapter, cathodic protection performance of TiO2 film was indicated under UV ray irradiation condition. Usually, ceramic coatings inevitably have various defects even when appropriate coating

RkJQdWJsaXNoZXIy MjM0NDE=