ICF100158OR FRACTROGRAPHY OF S.E.N. SOFT SOLDERED COMPOSITE LAMINATES MADE FROM 0.8 % CARBON MANGANESE STEEL UNDER PLANE STRAIN CONDITIONS M.R. SABAYO Department of Metallurgical Engineering, Mehran University of Engineering & Technology, Jamshoro Pakistan. ABSTRACT: An attempt has been made to discuss the design criterion of the composite materials at and during service conditions of engineering structures. The present work supports this and suggests a compromise between the properties of the materials such as strength and fracture toughness with pearlitic and martensic structures of composite laminates by using thin sheets of critical thickness in the form of laminate with crack divider geometry under plane strain conditions. This is supported by the load displacement graph by using an Instron testing machine at a strain rate of 0.05 cm/min and the fractography which supports the same modes of failure during fracture process. Thus suggesting the advanced materials for achieving the structure integrity of engineering structures. KEY WORDS: Composite laminates, crack controlling properties, delamination fracture and structural integrity. INTRODUCTION: A most serious problem now a days is to be able to build an Engineering structure which can resist the cracks or flaws present in it. Failure may take place in such structures below their yield or ultimate strengths. To over come this, composite materials, particularly laminates have been used, (Embury, (1), 1969). Such materials C not only resist crack propagation more (Sabayo, (2), 1981), than the homogenous materials but also have higher critical crack lengths giving a better chance of crack detention prior to failure and in some cases completely prevented through the thickness cracks (Sabayo, (3), 1982). This has drawn attention to the role of interfaces, their strength, delimitation during and after fracture, and the thickness of elements (layers) used in composite laminates. Crack controlling properties and lamination have recently been applied in conventional metallurgy. Steel can be made more resistant to crack by cementing together thin sheets of it with soft solder. This laminated steel is of course a composite materials, (Kelley, (4) 1970). Such studies have shown that through proper control of mechanical properties of the bonds, joining the sheets, it is possible to introduce delimitation fracture that markedly improve the over-all toughness of composite and in some cases completely prevented through the thickness cracks, (Sabayo, (5), 1983). In order to optimize the performance of the composite materials, it is necessary to gain some fundamental understanding of the nature of the components. Even for simple external composite loadings, the state of stress and strain at the interfaces between the components are complex and vary from place to place in the composite. This complexity of conditions at the interface is different from what might be expected from simple loading conditions. Although a precise description of the interface is beyond our present knowledge, and understanding of the role of the interface on composite behaviour and the ability to control the interface are important factors. (Sabayo, 5, 1991). Strength and toughness are related but different properties. One is generally obtained at the expense of the other where as the lamination provides a means of increasing resistance to fracture that is independent of the structure variables of the materials very much required for achieving the structural integrity. (Sabyo, 6, 1997).
RkJQdWJsaXNoZXIy MjM0NDE=