ICF10B

extending its applications in engineering, particularly where large deformation or thermal shock are unavoidable. Whereas the fatigue strength and the fatigue crack growth behavior of the metal matrix composites have been presented extensively in the literatures[2]-[5], limited results have been reported on the cyclic deformation of this type of materials, especially, at elevated temperature. The present study is to investigate the fracture behavior of a SiCw/6061Al composite and its matrix under cyclic loading. 2. MATERIAL AND EXPERIMENTAL PROCEDURES 2.1 Material and specimen The material used in the present study was a 6061 Al alloy matrix composite(MMC) reinforced with 22vol% SiC whisker, fabricated using a high pressure infiltration technique[2]. For comparison, a 6061 Al alloy(matrix) was also prepared in the same fabrication route as for (MMC). Both MMC and matrix materials were heat treated to the overaging conditions. Solid solution treatment was performed at 803K for 9ks followed by water quenching, then aged at 450K for 180ks to achieve overaged condition. The test specimens were machined with the loading axis perpendicular to the casting direction. The plate-shaped specimens of 80mm long, with gage section of 4×6×20mm, following ASTM (E606-92) recommendations were used for this study. The surface of the uniform-gage section of the specimens was carefully polished. 2.2 Testing procedures A servo-hydraulic testing machine (load capacity: 50kN) was used in the present study. The tensile tests were performed in stroke controlled mode in accordance with ASTM E8M at an average cross head speed of 10-2 mm·s-1. The cyclic deformation tests were performed in a fully reversed axial total-strain controlled mode. The strain rate was kept at 10-2s-1 for various strain amplitude tests. Since triangular wave was used for the strain controlled testing, a constant strain rate was available during the complete loading cycle. The cyclic stress-strain behavior was studied with the incremental step method at different temperatures. The tests were carried out typically with a initial total strain amplitude, ∆εt/2 of 0.075%. After 10 loading cycles, the total strain amplitude was increased by 0.075%, and the procedure was repeated. The tests were conducted in air at RT(293K), 373K, 423K and 473K. The specimens were heated in a resistance furnace with a temperature accuracy of ±1K, and kept at the testing temperature for 3.6ks before starting a test. 2.3 Microstructural analysis The fracture surfaces and gage section surfaces were examined in a scanning electron microscope (SEM), and an energy dispersive x-ray analysis system was used to determine the chemical compositions on some local area of fracture surfaces. Transmission electron microscope (TEM) was also used to study the microstructure of the specimens for different loading histories. TEM samples were sectioned near the fracture surface along the loading axis of the specimen. Ion-milling was utilized for the final thinning of the samples. 3. EXPERIMENTAL RESULTS AND DISCUSSION 3.1 Mechanical behavior Figure 1 shows the stress-strain curves of MMC under cyclic and monotonic(tensile) loading at different temperatures. It can be seen that the stress response of MMC under cyclic loading were higher that those under

RkJQdWJsaXNoZXIy MjM0NDE=