Metco 130, some cracks also propagate along splat boundaries (Figure 3b). However, in the nanocoatings with the bi-modal microstructure, there are various microstructural features that serve to arrest or deflect cracks and provide toughening. Figure 3c shows a crack being stopped or trapped in the partially melted region. Figure 3d shows a crack being deflected at the interface between the fully melted splat region and the partially melted spherical particles. It is well established that toughening mechanisms such as crack deflection and crack trapping can improve the crack growth resistance of brittle materials [5-8]. Thus, based on these results, we can conclude that nanocoatings should have higher crack growth resistance than Metco 130 coatings because of the toughening mechanisms observed in the nanocoatings. In order to provide a semi-quantitative determination of the effect of microstructure on crack growth resistance, the microstructural changes with CPSP were determined. Figure 4 shows that the volume fraction of the partially melted regions decreases with CPSP. Based on detailed examination of cracks around at least 10 hardness indentations in each nanocoating, the relative contributions made by various microstructural features, interface boundaries, porosity, partially melted and fully melted regions, to crack growth resistance was assessed. Figure 5 shows the results. By comparing Figures 4 and 5, it can be seen that at CPSP=410 where 90% of the microstructure is fully melted splats, the splats account for only 10% of the crack arrests. By contrast, 64% of the crack arrests in the CPSP=410 specimens are associated with crack arrests in the partially melted regions and by crack deflection at the boundary between partially and fully melted areas. Percent Partial Melting (Volume Percent) J J J H H H H H 0 10 20 30 40 50 60 290 310 330 350 370 390 410 Critical Plasma Spray Parameter H J Nano AT Mod. Nano AT 6000 7000 8000 9000 Plasma Torch/Particle Temperature (K) at z = 20 mm Figure 4. Percentage of coating that is partially melted, determined by quantitative image analysis as a function of CPSP or the plasma torch temperature at a spray distance of 20 mm.
RkJQdWJsaXNoZXIy MjM0NDE=