In the present work, finite element calculations were performed to determine in-service stress levels developed in a steel connecting rod of a high power diesel motor used for offshore oil well perforation. As surface cracks were found to be present, apparently due to inadequate maintenance, eventual failure of the rod by fatigue was considered to be a real possibility. With this in mind, the mechanics of surface cracks proposed by Newman and Raju [1] was adopted and a design curve depicting the relationship between the length and depth for nonpropagating semielliptical cracks was established. Using the same mechanics, growth kinetics and hence fatigue life were estimated for propagating semielliptical as well as semicircular cracks of different initial dimensions. FATIGUE LIMIT The connecting rod under consideration was made of a BS 818M40 high strength low alloy forged steel, with a yield stress, σY, and ultimate strength, σu, of 710 and 880MPa, respectively. As to the fatigue limit, this was estimated from [2,3] σe = kakbkckdσu /2 (1) ka, kb, kc and kd in the above equation are factors which take into account the effect, on the fatigue limit, of the degree of surface finish, size of the component, confidence limit and service conditions. For normal surface finish and ambient service conditions, it is proposed [2,3] that the factors ka and kd be taken as 0.9 and 1, respectively. The size factor kb which corresponds to the cross sectional dimensions (12 x 42mm) of the rod was estimated following [2] as 0.77. Finally, for a survival probability of 0.99, a confidence limit kc of 0.814 was adopted [2] and Eqn. 1 was then used to deliver a value of 248MPa for the fatigue limit of the rod. This value should be viewed as only a rough estimate of the steel's endurance limit, given the empirical nature of Eqn. 1. One may also add that Eqn. 1 is, in fact, valid for rotational (fully reversed) bending. STRESS CALCULATION The forces acting on the connecting rod during the operational cycle of the motor were estimated from appropriate data referring to both operational and dimensional aspects of the motor’s components. The inertia force, driving force and frictional force were taken into account and were assumed to be uniformly distributed over the areas on which they respectively act. The connecting rod was then modeled in the X-Y plane by a number of finite elements (Figure 1), with their third dimension (along the Z axis) corresponding to the rod thickness. An ANSYS 5.1 ED software was used and stresses were calculated for various positions of the rod during its operational cycle. The results obtained have indicated that the region between the holes in the above figure is the most highly stressed area and that stresses there vary between a minimum of zero (no load) and a maximum of about 300MPa. This gives rise to a cyclic loading of stress amplitude, σa, and a mean stress σm of 150MPa. The equivalent stress amplitude (σar) for a completely reversed loading can be calculated from [3] σar = σa/ (1 − σm/σu) (2) resulting in a value of approximately 180MPa, which is less than the fatigue limit, σe, estimated earlier. One may thus conclude that the connecting rod was in fact appropriately designed. However, the presence of surface cracks capable of propagating under the cyclic stress state acting in the rod can lead to its failure and the prediction of fatigue life in this case becomes a necessary undertaking. Establishing a size criterion for nonpropagating cracks, though, should precede such an undertaking.
RkJQdWJsaXNoZXIy MjM0NDE=