ICF10B

deformation is observed that manifests itself as a sharp change of load on tensile diagrams [1]. The effect of the ECP on the metal with non-conducting defects of the crack type would have shown up most vividly at a temperature of 4.2 K since in the zone adjacent to the crack tip the concentration of electromagnetic, thermal, and force fields reaches its maximum. Under conditions of subzero cooling (< 20 K) most metallic materials exhibit instability of plastic yielding that manifests itself in jump-like deformation (discontinuous yielding). The latter is recorded in the form of saw-tooth tensile diagrams. The initiation of the low-temperature discontinuous yielding and its character depend on a number of factors. One of the main factors is the volume of the material deformed. Strain constraint in the region of the material adjacent to the crack tip and nonmonotonic evolution of the plastic flow at cryogenic temperatures are responsible for specific features of the formation of the plastic deformation zone and the conditions of the evolution of fracture. It is the foregoing that determined the objective of the present investigation – to establish specific features of the evolution of plastic deformation at the crack tip related to the action of the ECP and cooling down to 4.2 K. EXPERIMENTAL RESULTS AND DISCUSSION For the investigation we have chosen steel 03Kh20N16AG6, which exhibits stability of the phase composition in the temperature range from 293 to 4.2 K. Compact tension (CT) specimens of 12 mm thickness were fabricated from sheet billets of that steel. Analysis of fracture diagrams of CT specimens obtained at the temperature of liquid helium revealed the appearance of local load maxima to the left of the 5 % secant. In this case, we face the uncertainty in the determination of the design load [2, 3] because these local maxima can be indicative of both crack growth onset and discontinuous yielding of the material that is characteristic of the steels considered at 4.2 K in the process of plastic zone formation at the crack tip preceding its growth onset. QP To verify this assumption, an experiment was performed according to the following scheme. Compacttension specimens of steel 03Kh20N16AG6 were loaded at a temperature of 4.2 K until several local maxima appeared located to the left of the point of intersection of the load displacement (P –V) diagram with the 5 % secant. Then the specimens were unloaded. A possible crack extension increment was controlled by thermal painting. Ten specimens were tested in this way and no crack extension was observed. It is only after the maximum that coincided with the point of intersection of the 5 % secant with the P – V diagram or immediately following it that the crack growth onset was noted. Thus, the presence of a number of local maxima on the P – V diagrams to the left of the 5 % secant in testing CT specimens of the above steel is a result of the formation of a plastic zone prior to the crack growth onset that, under these temperature conditions, occurs by the mechanism of discontinuous yielding. The formation of a plastic zone due to discontinuous yielding is also confirmed by the fact that the stress values corresponding to the beginning of discontinuous yielding and determined on smooth specimens coincide with the values of nominal stresses in the weakened section of the CT specimen, 0σ , under the load corresponding to the first local maximum . The value of σ is calculated by the following formula [3]: 1DP 0 ( ) ( ) , 3 1 1 0     − + + − σ = b l b l b l t PD (1) where t is the specimen thickness, b = t2 is the distance from the line of load application to the specimen edge; l is the distance from the line of load application to the crack tip.

RkJQdWJsaXNoZXIy MjM0NDE=