ICF10B

The stress of the beginning of discontinuous yielding determined on smooth specimens at a temperature of 4.2 K corresponds to the yield strength of the steel studied and is equal to 1440 MPa. The magnitudes of nominal stresses calculated by formula (1) for a batch of CT specimens are within 1400 – 1470 MPa. It is obvious that due to stress concentration in some region in the vicinity of the crack tip the stresses not only reach the level of the stresses corresponding to the beginning of discontinuous yielding, but exceed it. When studying the influence of the ECP on the kinetics of plastic zone formation at the crack tip, electric current pulses were applied so that the current flew about the crack tip. This direction of the current causes local concentration of the electric and thermal fields [1] and also contributes to elasto-plastic deformation of the largest region of the material at the crack tip. The maximum value of the current density with the consideration of its concentration at the crack tip with its pulse amplitude being equal to 2800 A reached 18.5⋅108 A/m2. The load levels, at which the specimens were exposed to the action of the ECP, produced nominal stresses equal to 0.6 0.2 σ , , and 1.2 0.2 σ 0.2 σ . Passing through the material at the nominal stress equal to 0.6σ0.2, the ECP does not change the run of the PV diagram and the character of crack propagation as compared to the initial state. The influence of the ECP at the nominal stresses σ0.2 and 1.25σ0.2 causes some deviation from the linear portion of the P-V diagram appearing as horizontal steps. However, the crack propagation is therewith not observed. At the same time, the first local maximum after the action of the ECP corresponds to the crack growth onset. The estimation of the plastic zone radius was performed on the basis of the Irvin approach [4] according to which nr 2 0.2 . 2 1       = σ π K p stress r in the case of the plane stress state, and 2 0.2 . 6 1       = σ π K p strain ECP p stress r . ( . ECP pr 1.15 r in the case of the plane strain state. The estimation showed that on the exposure to the ECP at the instant of the crack growth onset mm and ( mm). Also the values are matched by the values of the plastic zone radii ( calculated for the local maximum corresponding to the crack growth onset in the absence of the ECP action. Meanwhile, in the latter case for the first local maximum the size of the plastic zone radius is equal to 2.18...2.33 . = ECP p stress r 0.75...0.78 . ECP p strain r pr . ) .p strain r = stress ) strain 1.05... . = p stress r mm and mm, i.e., under this load the plastic deformation zone at the crack tip does not reach its critical size. 0.35...0.40 . = p strain r The fracture kinetics of steels at the initial stage at a temperature of 4.2 K and under the action of the ECP has also been studied by the method of stereofractographic analysis following the procedure described in [5]. Two batches of specimens were loaded in the medium of liquid helium. One part of the specimens of the first batch was loaded until the first clear-cut local maximum appears on the P-V diagram and then unloaded. The second part of the specimens was loaded until the appearance of two local maxima. The next batch of the specimens, which was divided into two parts, was exposed to the ECP and also loaded until the appearance of two maxima. The specimens of the second batch were unloaded as soon as the load reached the values corresponding to those attained in testing the first batch of the specimens. In this case, the only local maximum was observed at the load value corresponding to the appearance of the second local maximum for the specimens not exposed to the ECP. After unloading a possible crack extension increment was recorded and the specimens were fractured. Stereo pairs were photographed on the halves of the fractured specimen using a scanning electron microscope ‘Stereoscan’ at the convergent angle and magnification M=400. The stereo pairs were processed by a stereocomparator “Stecomoter”. 05 Θ=

RkJQdWJsaXNoZXIy MjM0NDE=