ICF10B

A similar analysis of the minor peaks appearing in the force-time records, including the one arising in the descending part of the first peak (see Figures 3 and 5) when specimen length, L, is increased, shows that they can be interpreted as the effect of higher modes of vibration. As a matter of fact their distance from the major peaks turns out to be in a constant ratio to the fundamental vibrational period (TAB). 0 100 200 300 Load (N) L/W=4.4 A B 0 100 200 300 Load (N) L/W=6.1 A B L/W=7.5 B A 0 100 200 300 0 0.2 0.4 0.6 0.8 1 Load (N) Time (ms) L/W=6.8 A B 0 0.2 0.4 0.6 0.8 1 Time (ms) L/W=8.6 A B Figure 5 – Example of a load-time traces recorded in one-point bending impact tests on specimens with a/W=0.5 and varying relative specimen length L/W 0 100 200 300 400 500 600 0 5 10 15 20 25 30 TAB (ms) ψ(a/W,L/W) Fig. 6 – Time interval between the first two main peaks A and B of load-time traces recorded on specimens of varying relative notch depth a/W and relative length L/W, as a function

RkJQdWJsaXNoZXIy MjM0NDE=