ICF10B

The methods for determining closing and opening force of fatigue cracks are Elber’s[8] and Brahmaf’s[9]test measurement methods and McCLung’s[10] FE calculation method. In this paper the test method is adopted to measure closing and opening force of SCT specimen. In the test we use tensiometer and load sensor to measure P-COD diagram of the specimen, as shown in Fig. 7. It can be seen from Fig. 7 that the slope of P~COD curve between point A and B is bigger than the ones of other section, indicating the rigidity of the specimen is biggest and the crack fully closes; the slope of the curve between point B and C gradually decreases, the crack gradually opens and fully open at point C; after point C, the slope of the curve presents linear feature. Therefore, records below point C of the curve indicate the cracks does not fully open until point C is reached, therefore, the force corresponding to point C is the opening force. Also from Fig. 7 it can be seen that the return process also has the similar case, yet the opening and closing forces are basically equal. The value for opening force, COD δ and crack length corresponding to this value measured in the test are acquired and recorded automatically by computer. The value of effective stress ratio U obtained through calculation is: p p p pop op U min max max min max max − − = − − = σ σ σ σ (12) U-a relation can be seen in Fig. 8. It can be seen from Fig. 8 that U values of the two specimens are bigger in the beginning, but they are quickly decreased to a certain value, and slowly increased to a stable value. The U value of prestretched specimen SCT6 is smaller than that of unprestretched specimen SCT7. When the crack propagates to a certain length, the U values of the two specimens gradually approach. At this time, crack has already propagated beyond the plastic zone of SCT specimen, the effect of prestretched plastic zone on crack closing has been eliminated. 4.3 Fatigue crack propagation rate Fig. 7 SCT specimen vs. P-COD curve Fig. 8 Effective stress ratio of SCT specimen Within the elastic zone, fatigue crack propagation rate can be calculated by Paris equation: m A K dN da ) ( = ∆ (13) Elastoplastic fracture parameter—COD δ is a simple and practical parameter, suitable for both elastic and elastoplastic conditions. The Paris equation is rewritten as follows after Δδ is taken as a fatigue parameter in the test: n B dN da ) ( δ = ∆ (14) Calculate COD as per formula (11). The da/dN~Δδ relation measured in the test are shown in Fig. 9, by regression, the Paris equation is obtained: 3 .21 ) 2 .683 ( δ ∆ = dN da (15) It can be seen from Fig. 9 that at the same Δδ, the fatigue crack propagation rate of prestretched specimen is smaller than that of the unprestretched one. When the crack propagates to a certain length, their propagation rates approach. The data are diversely scattered. For smaller cracks, the phenomenon of short cracks occur although da/dN decreases, Δδ increases. It can be regarded that this phenomenon is mainly attributable to the influence of crack closing effect. The presence of structural plastic strain zone makes the closing effect of the cracks more serious, resulting in reduction of Δδeff and slowdown of fatigue crack propagation rate. It can be seen from the effective stress ratio U (Fig. 8) that the U value of prestretched specimen SCT6 is lower than that of unprestretched specimen SCT7 due to existence of residual plastic zone. Therefore, production of residual plastic strain at the location of stress concentration such as the nozzle knee in conventional hydraulic test of pressure vessel is very favorable to reduction of fatigue crack propagation rate of these locations and extension of fatigue life. Make closing effect correction to Δδ: y eff eff E K σ δ 2 2 ∆ = ∆ (16) 5

RkJQdWJsaXNoZXIy MjM0NDE=