ICF10B

δ δ δ σ δ σ ∆ ∆ = ∆ ∆ = ∆ ∆ = − − = eff y eff y eff open E E K K K K K K U 2 2 max min max max (17) Δδeff~da/dN relation after taking into account the closing effect is shown in Fig.10. It can be seen from Fig. 10 that the two specimens have a good linearity for data and approach very much, which is expressed using unified fatigue crack propagation rate as follows: 2 .56 ) ( 5 .827 eff dN da δ ∆ = (18) The crack fatigue propagation rate of standard CT specimen of the same material is: 2 .06 ) 4 .905 ( eff dN da δ ∆ = (19) Fig. 9 da/dN-Δδ relation of SCT specimen Fig. 10 da/dN-Δδeff relation of SCT specimen It can be seen from the above equations that the fatigue crack propagation law of SCT specimen after closing effect correction is basically in agreement with the results of standard CT specimen. 5. CONCLUSION (1) FE calculation and measured results on test stress of SCT specimen successfully repeat the main characteristics of high strain of engineered construction such as pressure vessel nozzle, the simulation of high-strain zone of engineered construction is realized using small test specimen, and by changing the scale of geometric dimensions, opening diameter and shape of the specimen, it is convenient to change its stress-strain field, thus providing an effective and convenient tool for fracture and fatigue research of pressure vessel with nozzles. (2) Measured the plastic rotational factor of SCT specimen r=0.28, and measured the δ of COD by r and crack mouth opening displacement; (3) Measured the opening and closing force of fatigue cracks in high-strain zone of SCT specimen, obtaining the effective stress ratio U; (4) Proposed the engineering calculation method for COD in high-strain zone of SCT specimen and propagation rate of fatigue cracks corrected through closing effect, thus providing a basis for fracture and fatigue assessment of high-strain zone of pressure vessel nozzle. REFERENCE 1. Decock, J., Determination of Stress Concentration Factors and Fatigue Assessment of Flush and Extruded Nozzles in Welded Pressure Vessels, 2nd Int. Conference On Pressure Vessel Tech., Part 2, pp.821-834(1973) 2. Li Zezhen, Soloms G., Lucia A.C., Volta G., 1988, A Special Compact Tension Specimen for the Simulation of the Nozzle Corner Strain Field, Commission of the European Communities, JRC-Ispra establishment, 21020 Ispra, Italy 3. Chen Xuedong, Yang Tiecheng, Li Zezhen, Wang Zhaowei, Design Curves for Fracture Assessment in High-Strain Region of Pressure Vessel Nozzles, 9th International Conference on Pressure Vessel Technology, Sydney Australia 9-14 April 2000 4. Zeng Guangxin, Li Zezhen, The Two Basic Problems for the Defect Assessment Methods, Collection of Pressure Vessel Defect Assessment Materials (No.5). 5. Cai Cigung, 1979, Crack Propagation in Plastic Strain Zone, J. of Mechanics 6. Mercle, 1976, ASTM STP 536 7. Gao Zengliang, Li Zezhen, Research on Fatigue Propagation Law of Shaped Specimen Plate Simulating High-strain Zone of Pressure Vessel Nozzle, Zhejiang Industrial University Bulletin, No.4, 1985 8. Elber Wolf, The Signification of Fatigue Crack Closure, Damage Tolerance in Aircraft Structures. ASTM STP 486, American Society for Testing and Materials, 1971, 230-243 9. Barhma, K. Et al, Observation of Crack Closure Using a Crack Mouth Opening Displacement Gauge, Int. J. Fatigue, 1989.11(1); 37-41 6 10. McClung, R. C. And Sehitoglu, H. On the Finite Element Analysis of Fatigue Crack Closure -1, Basic Modeling Issues, -2 Numerical Results, Engineering Fracture Mechanics, 1989, 33, 217-272

RkJQdWJsaXNoZXIy MjM0NDE=