ICF10B

0.1 1 10 100 1000 0 0.02 0.04 0.06 0.08 0.1 0.12 0.14 Crack Velocity (m/s) T ε M( P am ) 7075 1st Experiment 7075 2nd Experiment Fig. 4. T*ε versus crack velocity. CONCLUSIONS The experimental evidences accumulated over the past six years suggest that T*ε integral is a material property characterizing stable and dynamic crack growth. Specifically: 1. T*ε resistance curve reaches a plateau with static and dynamic crack growth 2. Crack curves in the direction of vanishing T*2 ε and grows with T*! ε following the T*ε resistance curve. 3. A crack instability criterion based on the T*ε resistance curve was proposed and experimentally verified. 4. Dynamic T*ε value reached a constant value at terminal crack velocity. ACKNOWLEDGEMENT This paper summaries the cumulative efforts of the authors’ colleagues of the past ten years. In chronological order, they are: Drs. Y. Omori, Pratt and Whitney Company, J. Lee, Republic of Korea Air Force, L. Ma, United Technology Research Center, P. Lam, Orbital Sciences Corporation and M. T. Kokaly, Fatigue Technology, Inc. This research was supported by FAA Grant No. 92-G005 and ONR Contract N0001489J1276. REFERENCES 1. Stonesifer, R.C. and Atluri, S.N., On a Study of the ( ∆T) and C* Integrals for Fracture Analysis Under Non-Steady Creep, Engineering Fracture Mechanics, Vol. 16 (1982), pp. 769-782. 2. Brust, F.W., Nishioka, T., Atluri, S.N. and Nakagaki, M., Further Studies on Elastic-Plastic Stable Fracture Utilizing the T* Integral, Engineering Fracture Mechanics, Vol. 22 (1985), pp. 1079-1103. 3. Omori, Y., Okada, H., Ma, L., Atluri, S.N, and Kobayashi, A.S., T*ε Integral Under Plane Stress Crack Growth, Fatigue and Fracture Mechanics, 27th Volume, ASTM STP 1296 (1997), eds. P.S. Plasik, J.D. Newman, and N.E. Dowling, pp. 61-71. 4. Pyo, C.-R., Okada, H. and Atluri, S.N., An Elastic-Plastic Finite Element Alternating Method for Analyzing Wide Spread Fatigue Damage in Aircraft Structures, Computational Mechanics, Vol. 16 (1995), pp. 62-68. 5. Nishioka, T. and Yagami, H., Invariance of the Path Independent T* Integral in Nonlinear Dynamic Fracture Mechanics, with Respect to the shape of a Finite Process Zone, Engineering Fracture Mechanics, Vol. 31 (1988), pp. 481-491. 6. Narasimhan, R. and Rosakis, A.J., Three-Dimensional Effects Near a Crack Tip in a Ductile Three-Point Bend Specimen: Part I—A Numerical Investigation,” ASME Journal of Applied Mechanics, Vol. 57 (1990), pp. 607-617. 7. Okada, H. and Atluri, S.N., Further Study on the Characteristics of the T*e Integral Plane Stress Stable Crack Propagation in Ductile Materials, Computational Mechanics, Vol. 23 (1999) pp. 339-352. 8. Cottrell, B. and Rice, J.R., Slightly /curved or Kinked Crack, International Journal of Fracture, Vol. 10 (1980), pp. 155-169. 9. Sumi, Y., Nemat-Nasser, S. and Keer, L.M., On the Crack Path Stability in a Finite Body, Eng’g Fracture Mechanics, Vol. 22 (1985), pp. 759-771 10. Nishioka, T., Sakai, K., Murakami, T. Matsuo, S. and Sakakura, K., Measurement of Nonlinear Fracture Parameter T Integral under Impact Loading Using Laser Caustic Method, Transactions of 11th International Conference on Structure Mechanics in Reactor Technology, G13/1 (1991), Tokyo, pp. 321-326. 11. Lee, J., Kokaly, M.T. and Kobayashi, A.S., Dynamic Ductile Fracture of Aluminum SEN Specimens: An Experimentalnumerical Analysis. International Journal of Fracture, Vol. 93 (1999), pp. 39-50. 12. Kokaly, M.T., Lee, J. and Kobayashi, A.S., Dynamic Ductile Fracture of 7075-T6 – An Experimental analysis, to be published in the International Journal of Solids and Structures. 13. Kobayashi, A.S. and Engstrom, W.L., Transient analysis in fracturing aluminum plates, Proceedings of 1967 JSME SemiInternational Symposium, JSME (1967), pp. 172-181.

RkJQdWJsaXNoZXIy MjM0NDE=