causes the crack initiation more easily [7]. The increase in compressive residual stresses and tensile strength might compensate for the reduced fatigue resistance due to softening by retained austenite. Since the maximum stress in a bent strip is on its top surface, the bending fatigue strength is mainly dependent on the surface conditions and its strength. In spite of the fact that the compressive residual stresses and the tensile strength were increased with the increase of retained austenite, no continuous increase in the bending fatigue strength was obtained. This might also be attributed to the presence of retained austenite. The earlier experiences [7, 8] show that due to its weakness and easily slipping the presence of retained austenite near the top surface will facilitate the crack initiation during bending cyclic loading. In this investigation, however, very fine elongated retained austenite (about 0,1µm) was observed to have been embedded between two acicular martensite phases [2]. This might reduce the risk of retained austenite for crack initiation, and may also give an explanation why high bending fatigue strength can still be maintained in the material with large amount of retained austenite (14,3vol%). CONCLUDING REMARKS Increase in the strength or hardness of the material was the additive of the precipitation strengthening of fine dispersed M23C6 and Fe3C particles and the softening due to the increase of retained austenite. It reached a maximum value at about 10vol% retained austenite. The impact fatigue strength was significantly improved with increasing retained austenite. The presence of retained austenite however had little influence on the fatigue strength in tension. For the bending fatigue strength, it increased with increasing retained austenite and reached a maximum value at about 4 % retained austenite. Increase in impact fatigue strength was likely attributed to the increase in its ability for impact energy absorption (damping capacity and plasticity) by increasing retained austenite and its tensile strength by precipitation strengthening. For fatigue in tensile, crack initiation at inclusion was the main fracture mechanism. For fatigue in bending, the presence of retained austenite near the top surface may facilitate crack initiation. High bending fatigue strength maintained in the material with large amount of retained austenite was owing to its high tensile strength and fine dispersed retained austenite. ACKNOWLEDGEMENTS This paper is published by permission of AB Sandvik Steel. The support of Dr T. Thorvaldsson, Mr H. Holmberg, Mr M. Lundström, and Mrs M. Sundqvist, and the technical assistance of Mr G. Svensk, Mr D. - E. Gräll, and Mr C. Lundemo are gratefully acknowledged. REFERENCES 1. Olsson, S. (1992). In: Proc. of the 1992 Inter. Compressor Engineering Conf. at Purdue, pp. 909-918, Hamititon J. F. (Eds). Purdue University. 2. Nyström, M., Liu, P., Larsson, T., Olsson, S. and Svensk, G. (1996). In: Proc. of the 1996 Inter. Compressor Engineering Conf. at Purdue, pp. 511-516, Soedel, W. (Eds). Purdue University. 3. Svenzon, M. (1976). Ph. D Dissertation, Uppsala University, Sweden. 4. A guide for fatigue testing and the statistical analysis of fatigue data, ASTM Special Technical Publication No. 91-A, 1963. 5. Jun, J. and Choi, C. (1999). J. Mater. Sci., 34. 3421. 6. Yu, J., Liaw, P. K. and Huang, M (1999). JOM, Apr. 15. 7. Inada, I., Hiroshi, Y. and Tsuyoshi, I. (1994). Kobeco Technology review, 17, 49. 8. Kumagaya, S. (1975). Metals in Engineering, 15, 15.
RkJQdWJsaXNoZXIy MjM0NDE=