ICF10B

In this presentation we will mainly deal with polypropylene (PP), which shows an extraordinary breadth of fracture phenomena (brittle fracture through unstable rapid crack propagation, slow creep crack growth, crazing or macroscopically homogeneous deformation leading to plastic instability). The mode of fracture is largely determined by the competition between stress transfer onto backbone chains and the intensity of the different relaxation mechanisms, including segmental slip and disentanglement, void formation and chain scission. The inherent ductility and low glass transition temperature, Tg, of PP give rise to strongly rate dependent local plasticity effects, which have to be taken into consideration for a quantitative evaluation of toughness. In the following we will briefly indicate the molecular and structural origins of the different deformation and damage mechanisms. Their effect on fracture toughness will then be assessed using three methods (J-Integral, EWF, LEFM). DEFORMATION AND DAMAGE MECHANISMS AND THEIR EFFECT ON FRACTURE BEHAVIOR Semi-crystalline polymers are highly heterogeneous on a molecular and microscopic scale. The smallest building-blocks considered here are aggregates of crystal lamellae connected by amorphous regions. These latter consist of a network of non-extended entangled chains, dangling chain ends and/or loops, and more or less taut tie-molecules. When a spherulitic sample is strained, local strains within a lamellar stack will vary considerably, depending on the local Young's modulus, the relative orientation of the lamellar stack with respect to the principal stress direction and the modes of stress relaxation available to a given volume. Above Tg the amorphous regions will account for most of the elastic and anelastic deformation. The regions oriented perpendicular to an applied (uniaxial) stress will initially mainly deform by interlamellar separation. Evidently, the difference between the crystalline and amorphous moduli and the resulting strain concentration become relatively small at T<<Tg. Crack extension in this temperature range occurs by rapid straining and failure of the material ahead of the crack tip following the plane of least resistance, i.e. generally through and along the amorphous interlayers. Tie chains are stretched and broken rather than pulled out. Thus, plastic deformation of the bulk material is relatively limited and crack resistance is well quantified by the critical strain energy release rate GIc (or by the critical stress intensity factor KIc) using the standard methods of Linear Elastic Fracture Mechanics [2, 3]. More extensive anelastic and/or plastic deformation is observed if the drawing process also involves the crystalline regions. Homogeneous, ductile deformation through lamellar shear is favored by intense stress transfer between crystal lamellae through strong, well-entangled amorphous regions and a large concentration of tie-molecules. These parameters also increase KIc. On the other hand, low molecular weight and rigid crystal lamellae favor heterogeneous, localized deformation leading to craze-like features and brittle fracture [4]. However, the mode of fracture is not an inherent property of a given material, it depends strongly on temperature, time scale and state of stress. For an unmodified high molecular weight polypropylene (PP) it changes as a function of loading rate v from full shear yielding (v < 1 mm/s) to small scale yielding and multiple crazing (10 mm/s – 1m/s) and to formation of a single crack (v > 2 m/s) [5]. The time scale is evidently shifted with molecular weight and temperature (see below). FRACTURE MECHANICAL CHARACTERIZATION Essential Work of Fracture (EWF)

RkJQdWJsaXNoZXIy MjM0NDE=