Figure 1: SEM images of the overall appearance of the fracture surfaces. In order to confirm the above macroscopic observations, higher magnification images of the fracture surface are required. In Figure 2, a SEM image of from fracture surface of the specimen loaded along the [100] orientation demonstrates markings typical of cleavage fracture. Figure 2: SEM image of the fracture surface of the [100] crystal aged 1.0 hr @ 773 K. As such, it is confirmed that the NiTi crystals undergo local material cleavage in some regions of the specimen. The markings in Figure 2 have facets on the {100} planes, with crack growth along the [011] direction and a crack line along the [011] direction. We note that the observed cleavage planes have a correspondence to the highly symmetric B2 parent phase rather than any relation to the habit planes of the low symmetry Type II B19’ martensite plates, (-0.88, 0.21, 0.40). Such an observation circumvents any relation between the propagation of overload cracks